Meaning
A purge is resin pumped through the barrel and nozzle to clear the previous material or degraded melt before molding resumes. It is also the material used for the job. A molten purge doubles as a test sample for acetal. Purging is part of every start, color change, long stop and shutdown.Purge Resins
DuPont picks polystyrene, cast acrylic with the nozzle removed and high density polyethylene. They stay stable over a wide temperature range and leave other polymers alone. The procedure pulls the unit back and runs the screw fast to pump out the old resin. Purge resin is fed until the output is clean. Several fast air shots then scrub the cylinder walls.Read More
Foaming Test
DuPont drops a molten acetal purge into water. Sound melt carries no gas bubbles, is denser and sinks, and its section shows only the matte voids of crystallization. Degraded melt carries bubbles and floats, with large shiny voids from degradation gas. The test is run on the purge before the first part is kept. It is especially useful with colorants, some of which degrade acetal.Long Stops
On a short stop the melt is lowered to 30 °C (60 °F) below the recommended value and air shots are fired. A long stop calls for a purge with high density polyethylene or polystyrene. At shutdown the hopper is closed, the barrel is emptied and purged, and the screw is left forward.Covestro Practice
Covestro asks for a purge before production with its thermally conductive polycarbonate. The viscous, hot melt can lift deposits left by the previous material.Acetal Precaution
A barrel or hot runner that last ran PVC or a flame-retardant grade is cleaned before acetal runs in it.