A DuPont wear-test sample part in acetal measured 49.61 mm on its outside diameter with a spread of ±0.02 mm after 15 seconds of packing and only 2 seconds of cooling in the mold. The same part molded with the same 15 seconds of packing and 15 seconds of cooling measured 49.76 mm with a spread of ±0.07 mm. Longer in the tool meant a larger, looser part, and the shorter stay gave a smaller, tighter one.
That table runs against the habit of adding cooling time to be safe. After the cavity fills, three clocks run in sequence: the pack pressure that feeds the cavity while the melt shrinks, the hold time that keeps it feeding until the gate freezes, and the cooling time that ends at ejection. Each has a way of being found by measurement, and each has a cost when it is set by habit. This piece follows them in order, with the weight studies and cooling data that resin makers and one journal paper publish.
What Pack Pressure, Hold Time and Cooling Time Each Do
Fill is a speed-controlled move, and the pack phase is a pressure-controlled one. When the screw switches over, the cavity is full of melt that is already cooling against the walls. As the plastic contracts, more melt has to enter through the gate to replace the lost volume, and the screw holds a set pressure to push it in.
Pack pressure sets how much material is added. Hold time sets for how long it can be added, which ends when the gate freezes and no more can pass. After that point the part is sealed, and what remains is cooling, which is the time the part spends in the mold until it is stiff enough to leave without distortion.
DuPont’s nylon guide states the first two plainly. Pack pressure should be constant over the pack phase, and the correct hold pressure time is easy to find on the press by weighing parts. For a highly crystalline resin, the Delrin tips sheet adds that for a highly crystalline resin an adequate packing time secures both part performance and shot-to-shot dimensional consistency.
Pack and hold control the volume in the cavity; cooling controls the shape the part holds when it leaves. A short pack cannot be repaired with a long cooling time.
Why a Crystalline Resin Loses Volume While It Freezes
Delrin gives the clearest numbers. DuPont puts its crystallinity near 60 %, among the highest of any semi-crystalline thermoplastic. The melt weighs 1.17 g/cm³ and the solid 1.42 g/cm³, an 18 % gap. On the sheet’s PVT diagram 11 % of the volume loss comes from crystallizing and a further 7 % from thermal shrinkage, about 2 % in linear terms.
The 11 % is the part a pack phase can replace, because melt can still enter while the polymer crystallizes. Thermal contraction takes the other 7 %, after that point, and it happens to every part as it cools. DuPont’s point is that when packing replaces the crystallization loss properly, the remaining thermal shrinkage is independent of the part’s thickness, which means a part with thick and thin areas shrinks evenly.
Poor packing shows in the part. The sheet reports that poor packing in a narrow gate degrades mechanical performance by up to 30 %, adds warpage and leaves shrinkage uncontrolled. For a buyer reading a first article report, a part that is light against its sister parts is more likely to be under-packed than to have a measurement error.
Finding the Hold Time With a Part Weight Study
A part weight study is a short, inexpensive test, and it replaces guessing. DuPont’s guide gives the method for nylon, and it works for most semi-crystalline resins.
- Set a constant total cycle time for the whole study, so that the melt temperature does not drift.
- Mold parts at hold times 0.5 to 1.0 seconds apart, depending on the resolution wanted.
- Remove the runner and sprue from each shot and weigh each part on a laboratory balance.
- Plot weight against hold time and find the point where the weight first reaches its maximum.
The correct hold time is the first one that gives maximum weight. According to the guide, shrinkage reaches a minimum at the same hold time, so a dimensional check on those parts confirms the weight reading. Beyond that point more hold time adds nothing, because the gate has frozen, and it takes cycle time from the line.
Part thickness moves the answer more than most buyers expect. DuPont’s Delrin sheet shows optimum packing time and part thickness as a curve that is not linear. As thickness grows, the packing time needed per millimeter also grows. A rib 2 mm thick and a boss 6 mm thick do not just need three times the hold; the thick section needs a disproportionate share.
The weight study finds the shortest hold that fills the part. Any hold beyond it is waiting for the cooling time to catch up, and any hold short of it is a part that is not full.
The study also tests the tool. If the weight never plateaus, the gate is freezing before the part is packed, and the correction is at the gate, not at the machine. The next section gives the gate figures that resin makers publish.
How Hold Pressure Moves Shrinkage
Hold pressure is the second setting that the weight study fixes. For nylons, DuPont recommends the highest possible holding pressure to reduce mold shrinkage, usually around 90 MPa, and states that a variation of 10 MPa changes shrinkage by about 0.1 %. A press that cannot hold pressure steady within a few MPa will not give a stable shrinkage, whatever the drawing says.
One setting is used for the whole hold time. The guide says it is essential that a single pressure setting is used over the entire hold pressure time, because a changed pressure can leave non-uniform crystallinity in the part and lower mechanical properties.
Hold pressure and part thickness work together on shrinkage. DuPont’s charts for unreinforced nylon 66 show shrinkage falling as hold pressure rises, and rising with part thickness at a fixed mold temperature and pressure. Shrinkage also grows with mold temperature, since a slower cooling rate gives more crystallization before the part freezes. The same guide notes that parts molded cold show higher post-mold shrinkage and may carry severe internal stress, which can lead to premature failure.
| Setting | Direction | Size of effect given | Source |
|---|---|---|---|
| Hold pressure | Higher pressure, less shrinkage | About 0.1 % shrinkage for 10 MPa near 90 MPa | Zytel and Minlon guide |
| Hold time | Longer until gate freeze, then no change | Weight reaches maximum and shrinkage a minimum at the right time | Zytel and Minlon guide |
| Mold temperature | Hotter mold, more mold shrinkage, less post-mold shrinkage | Shown for a 3 mm part at 90 MPa | Zytel and Minlon guide |
| Part thickness | Thicker part, more shrinkage | Shown at 70 °C mold and 90 MPa | Zytel and Minlon guide |
| Packing time (acetal) | Optimum gives highest weight and lowest warpage | 15 s in a trial part | Delrin tips |
The Gate as the End of the Hold Phase
The gate sets how long the hold can work. For nylon DuPont sets the aim as a gate that closes just as the part finishes crystallizing, not ahead of it. A gate that freezes early seals a part that is still shrinking, and a gate that stays open too long is lost cycle time.
Geometry controls the freeze. DuPont gives gate thickness at 50 to 75 % of part thickness and a land length under 1 mm for nylons. For acetal it names the tunnel gate and gives four rules: place it in the thickest section, give it a diameter of at least half the part thickness, keep its length under 0.8 mm (0.03 in), and size the tunnel beside it at the part thickness plus 1 mm or more. A conical gate suits amorphous resins, but a crystalline one freezes in its narrow tip before packing ends.
Semi-crystalline and amorphous resins differ in where the failure shows. The Delrin sheet explains that a poor process leaves an amorphous resin over-packed and a semi-crystalline one under-packed and shrinking too much. Both need a weight study, but the amorphous resin shows its error as flash and stress near the gate, and the crystalline resin as sink, voids and size.
An aluminum bridge tool adds a thermal factor. The gate region of an aluminum tool loses heat faster than steel, since aluminum conducts 4 to 5 times as well as P-20 steel according to Arconic, and a gate that stays open in a steel tool can freeze sooner in an aluminum one. A weight study done on a different tool does not transfer, and one done in the bridge tool should be repeated if the tool is later moved to a steel cavity.
Cooling Time, Wall Thickness and the Tool Material
Cooling time is calculated for quoting and measured for running. K. A. Stelson’s paper in the Proceedings of the Institution of Mechanical Engineers reviews the published cooling time formulae for injection molding and finds that many contain errors, though they have been accepted for decades.
The abstract adds that ejection criteria can be based on either mid-plane or average temperature, and that thin and thick parts deviate from the theory’s assumptions. A formula is a starting point and the press gives the final number.
Wall thickness is the main variable, because heat has to travel from the middle of the part to the cavity wall through plastic that conducts poorly. DuPont notes that thick parts cool far slower than thin ones, a consequence of how poorly thermoplastics conduct heat. Covestro’s thermally conductive polycarbonate reverses part of this, since a conductivity of 8 W/mK or more moves heat out of the part and into the tool, which then sticks if the tool is too warm.
The tool material sets how fast heat leaves the cavity wall. Aluminum and copper alloys carry far more heat than tool steel, and Table 2 lists the values thyssenkrupp prints for common mold materials, converted to SI.
| Material | Conductivity, W/mK | Conductivity, Btu/ft/hr/°F | Expansion, 10⁻⁶ per K | Expansion, 10⁻⁶ per °F |
|---|---|---|---|---|
| QC-10 aluminum | 159 | 92 | 24.7 | 13.7 |
| 7075-T651 aluminum | 130 | 75 | 23.6 | 13.1 |
| P-20 steel | 29 | 17 | 12.2 | 6.8 |
| H-13 steel | 28 | 16 | 10.8 | 6.0 |
| 420 stainless | 22 | 13 | 11.2 | 6.2 |
| MoldMAX LH beryllium copper | 156 | 90 | 17.5 | 9.7 |
| PROtherm beryllium copper | 251 | 145 | 17.6 | 9.8 |
The MoldMAX brochure for its copper alloys claims conductivity up to ten times that of tool steel and cycles shorter by 15 to 50 %. It prints a comparison of mold cooling time, 10 seconds for a MoldMAX HH tool with the part at 92 °C, against 25 seconds with the part at 99 °C for the comparison tool. The maker states those figures for its own alloy in its own test, so they show the direction of the effect and not a promise for a given part.
A conductive tool changes the cooling time but not the hold time. The gate still freezes when the plastic there is crystallized, and a faster-cooling tool moves that moment earlier. Repeat the weight study when the cavity material or the cooling circuit changes, and treat any figure from another tool as a guess.
A buyer reading a trial report can use the same logic as a check. Any report that lists hold time without the part weights behind it, or cooling time without the date and conditions of the dimensional check, has skipped the two measurements that make the numbers repeatable. Ask for the weight plateau and for the measurement time and temperature, and treat a round number with no data behind it as a guess.
Ejecting Hot or Ejecting Cold
Whether a part needs cooling in the mold depends on the resin. DuPont’s nylon guide holds that crystalline nylon needs no separate cooling once the hold time has finished the crystallization, because the part is already stiff enough to eject. The Delrin sheet turns this into a rule for acetal: after adequate packing, let the part leave hot and cool in the open.
The reason is even shrinkage. A part has to shrink evenly without constraint while it cools, the sheet says, and an amorphous resin, which needs a long cooling time before ejection, ends with a longer total cycle than acetal. Ejecting onto a conveyor is preferred to ejecting into a box or bag, since a bulk container creates a temperature gradient through its height and may cause dimensional differences from part to part.
Table 3 gives the four trials of the wear-test part that opened this piece.
| Trial | Packing time | Cooling time | Cycle time | Outside diameter |
|---|---|---|---|---|
| 1 | 5 s | 24 s | 39 s | 49.48 ± 0.2 mm (1.948 ± 0.008 in) |
| 2 | 10 s | 7 s | 26 s | 49.48 ± 0.7 mm (1.948 ± 0.028 in) |
| 3 | 15 s | 2 s | 26 s | 49.61 ± 0.02 mm (1.953 ± 0.001 in) |
| 4 | 15 s | 15 s | 41 s | 49.76 ± 0.07 mm (1.959 ± 0.003 in) |
Trial 3 gives both the shortest cycle and the tightest spread, and trial 4 shows that adding cooling to a fully packed part held it in the mold while it shrank, with a spread of ±0.07 mm. The sheet describes the effect as uneven shrinkage with visible and measurable warpage and deformation. Its best-practice list adds that process settings should not be bent to chase dimensions, and that gate design and process conditions are checked before the cavity is corrected.
The rule is for crystalline resins. An amorphous resin such as polycarbonate needs time in the mold to become stiff, and it is in the amorphous case that the cooling circuit and mold material matter most.
Sticking, Undercuts and Ejection Faults
A part that will not leave the tool is a tooling problem with a process component. The tables above give the process side, and the faults below show how to separate the two.
- A part that sticks to the cavity half instead of the core is a draft, polish or temperature problem. DuPont recommends 0.5° to 1° per side for ribs, bosses and sides in nylon, with up to 2° for softer, more elastic resins.
- A part that sticks and leaves residue is often a mold that is too warm. Covestro says a mold temperature over its suggested range can delaminate its conductive polycarbonate slightly, and suggests 65 to 82 °C (150 to 180 °F), with beryllium copper at ribs and deep cores and different temperatures on the two mold halves to hold the part on the chosen side.
- An internal undercut that deforms on ejection may release with a hotter mold or a shorter cycle, according to DuPont, and an external undercut with a longer cycle and higher shrinkage. DuPont advises against undercuts above 3 % in glass-reinforced nylon, which has low elongation.
- A part with sink or voids is a hold problem. Check the weight plateau before changing the tool.
Cooling circuits belong to the same review. Arconic notes that aluminum’s conductivity calls for thermal isolation of a hot runner, and the same property moves heat out of the cavity. The records of the weight study, the cooling trials and the ejection settings go to the buyer with the first samples, and a supplier of low-volume injection molding that hands them over makes bridge production repeatable on a second press.
Sources and Further Reading
- DuPont, Molding tips to optimize production of components made with Delrin acetal homopolymer, Delrin Technical Guide
- DuPont, Zytel and Minlon nylon resins molding guide (GNE-A11218)
- K. A. Stelson, Calculating cooling times for polymer injection moulding, Proceedings of the Institution of Mechanical Engineers, Part B, 217(5), 709-713, 2003 (abstract page, University of Minnesota)
- thyssenkrupp Materials NA, Aluminum and copper mold materials for the plastics industry, CBS 017-04-18
- voestalpine High Performance Metals, MoldMAX plastic tooling alloys brochure
- Covestro, Processing information for Makrolon TC polycarbonate grades, COV-202, August 2022
- Arconic, QC-10 mold material, hot runner integration technical fact sheet