P-20

P-20 is a prehardened mold steel, at 26 to 34 HRC in the thyssenkrupp table, that serves as the steel reference for aluminum tooling.

Every P-20 article of the Injection Molding Resources, newest first, each written from published standards, research and makers’ data.

Meaning

P-20 is a prehardened mold steel, at 26 to 34 HRC in the thyssenkrupp table, that serves as the steel reference for aluminum tooling. Aluminum mold alloys are compared against it for conductivity, expansion and strength. It is harder and stronger than aluminum and conducts heat far less. A bridge tool in aluminum is judged by how it differs from P-20.

Conductivity

thyssenkrupp gives P-20 a conductivity of 29 W/mK (17 Btu/ft/hr/°F). QC-10 aluminum reaches 159 W/mK (92 Btu/ft/hr/°F). Arconic puts aluminum at 4 to 5 times the conductivity of P-20. An aluminum tool therefore pulls heat from the melt faster at a given mold temperature. Settings carried over from a steel tool are rechecked on the first shots in aluminum.
Read More

Expansion

P-20 expands at 12.2 × 10⁻⁶ per K (6.8 × 10⁻⁶ per °F). QC-10 expands at 24.7 × 10⁻⁶ per K, about twice as much. A hot runner fixed in an aluminum plate has to be designed for that difference.

Strength and Hardness

P-20 has a yield strength near 896 MPa (130 ksi), about two thirds above a QC-10 plate. MoldMAX lists P-20 at 30 HRC and H-13 at 45 to 50 HRC, while aluminum alloys sit on the Rockwell B scale. The scales do not compare digit for digit, but the ranking is plain. Aluminum is the softest cavity material and hardened tool steel the hardest.

Cycle Effect

In a cooling time table, P-20 sits beside H-13 at 28 W/mK and 420 stainless at 22 W/mK. The aluminum and copper alloys sit far above all three. A conductive tool shortens the cooling interval but not the hold time, because the gate still freezes when the plastic there freezes.

Mold Maintenance and Spare Inserts Across a Bridge Injection Molding Run

How a bridge mold is cleaned, inspected and fitted with inserts across a run, so that wear is recorded, predicted and met with spares instead of stoppages.

What a Bridge Mold Needs Between LotsThe aluminum maintenance column is plain on the first rule: an aluminum mold is taken apart and cleaned thoroughly after every run of parts, and cleaned again before storage, however short the run. It can often run five to seven days before it needs cleaning, the author notes, though some resins and some molds with actions need it after two to three days.

Draft Angle by Texture Depth on Injection Molded Parts

How much draft a textured wall needs for its depth, under which conditions each published figure holds, and how the mold and the part are checked.

How Much Draft a Texture Depth NeedsStandex Engraving Mold-Tech's technical data sheet gives the current recommendation from the texture maker: 1° of draft for every 0.013 to 0.015 mm (0.0005 to 0.0006 in) of texture depth. Per 0.025 mm (0.001 in) that works out to between 1.7° and 2°.

How Many Parts One Aluminum Injection Mold Gives

A mold's life is a toolmaker's rating for a stated resin and cavity count, converted into parts per tool and then into tools per quantity.

What Sets the Number of Parts One Aluminum Mold GivesThree things set it, and they act together. One is the alloy and where in the plate the cavity sits.

Cycle Time and Parts per Hour in a Bridge Injection Molding Run

A cycle is the sum of fill, hold, cooling and press motions, and a supplier's number is only as good as the pack and cooling times behind it.

What Sets Cycle Time and Parts per HourA molding cycle is a loop of seven moves: the mold closes, the cavity fills, the pack and hold phase runs, the part cools, the mold opens, the part is ejected, and the screw recovers for the next shot. Recovery runs while the part cools, which is why DuPont's nylon guide asks for screw speeds adjusted so that screw retraction time is shorter than the cooling phase.

How to Start Up an Injection Mold and Take the First Shots

A new mold is started cold on purpose, filled in stages with short shots, and read for vents, gates and heat before any process is fixed.

The Start-Up Sequence from a Cold Barrel to the First ShotEight moves take a machine from cold to its first complete part. The first four prepare the melt, the next three shape the shot, and the last one is a decision: whether the part describes the tool or only the settings.

Drying Resin and Setting Melt Temperature Before the First Injection Molded Part

Pellets are dried to a measured moisture limit, held there to the hopper, and melted inside a window that the resin maker prints.

What Dry Resin and a Correct Melt Temperature ProtectWater in a nylon melt is not a surface problem. DuPont explains that water carried into the melt triggers hydrolysis, which breaks the polymer down, costs toughness and strength, and makes the melt flow more easily.

Request an Injection Molding Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Injection Molding chosen.

Request a Quote