Two tunnel gates in the same mold, one 0.76 mm (0.030 in) across and the other 0.69 mm (0.027 in), differ by 0.08 mm (0.003 in). Jim Fattori uses the pair in Plastics Technology to make a point about percentages: the smaller hole has lost about a fifth of its flow area, and the cavity behind it may show sink or voids because its gate froze first. The part drawing shows neither gate, yet the two cavities will not make the same part.
The gate is where the melt enters the cavity, and it is also the last place the melt can be pushed from. Its position decides how the part fills, where the weld lines fall and how the part shrinks and warps. Its size and the time it takes to freeze decide how well the part is packed. This piece sets out what the resin makers, the simulation maker and the molding columnists publish on both questions, and how a hold time is found from the gate rather than guessed.
How Gate Location and Gate Freeze Shape a Molded Part
Autodesk’s Moldflow design rules open with the claim that gate position strongly affects material orientation and warpage, and that changing the gate is sometimes the only way to control orientation. Every gate injects under the same pressure, and the aim of gating is to avoid overpacking some paths while others are still filling, because unequal packing gives unequal shrinkage.
Gate freeze is the second half of the same story. While the gate is open, holding pressure keeps feeding melt into the cavity to make up for shrinkage. Once the gate has frozen, nothing more enters, and the part cools with whatever mass it holds. A gate that freezes too early leaves a thick section underpacked. A gate that stays open while the pressure is released lets melt flow back out.
Location decides how the part fills and shrinks. Size and freeze time decide how much melt it holds when the gate closes.
Where the Gate Goes on the Part
Joe Henz’s Plastics Technology column calls gate location the root cause of many molding difficulties and argues that the part designer, not the mold maker, should choose it. His two examples are simple. A long, narrow part that has to be straight is gated at one end, and a round part that has to be round is gated in the center. Many parts can absorb 0.13 to 0.38 mm (0.005 to 0.015 in) of bow or out-of-roundness, and those that cannot need the gate placed with that in mind.
Moldflow’s rules give the reasons behind those examples. A central gate gives equal flow lengths to every edge, so packing is even in all directions and the shrinkage difference is small. A long part gated in its middle packs heavily near the gate and orients the molecules or fibers differently along its length, which warps it. Gated at one end, the same part has uniform orientation along its length, and the packing difference from end to end does not bend it.
The rest of the rules read as a checklist:
- Gate into the thickest section, so the melt flows from thick to thin and the thick region receives the best packing. Gating into thin sections can cause hesitation, sinks and voids.
- Keep the gate away from load-bearing areas, because high pressure and velocity at the gate leave it highly stressed.
- Place the gate where its scar can be hidden or disguised.
- Place it so that air can escape, because unvented air gives short shots, burn marks or high pressure near the gate.
- Place it so that weld lines form early in filling or in a high-pressure area, where they meld well, and away from loads and visible faces.
Henz shows what happens when the weld line rule is ignored. A small 20 % glass-filled PBT part was given two gates by its mold maker, the gates formed a weak weld line in the middle of a highly stressed section, and the part failed. With one gate at the end, it worked as designed. His second case is a fan shroud gated in the center under a logo, which put a weak weld line across every vertical louver.
The resin makers repeat the thickest-section rule for their own materials. DuPont’s Zytel guide adds that gates are highly stressed areas and should not sit in mechanically critical areas. The Delrin molding guide puts gate position in the thickest area at the top of its tunnel gate criteria.
How Many Gates a Part Needs
Moldflow’s page on the number of injection locations says there is no fixed rule, then gives the factors. Thicker walls let the melt flow further. Each material has its own flow length for a given wall, printed on its datasheet. Large parts, thin walls and viscous materials need more gates.
Its method is to try one gate at the flow centroid first and check that every flow path fills at nearly the same moment. If one gate cannot meet that, the part is divided in thought into sub-moldings, each gated at its own centroid or at the middle of one side, with the runner sized so that all of them fill together. Where thick and thin sections sit side by side, the gate goes nearer the thick ones, so that the material between gate and thick region does not freeze before the thick region is packed.
More gates are not always better. Henz’s PBT part needed one gate and failed with two. Every extra gate adds a weld line where two flow fronts meet, so the count is a trade between flow length and weld line position.
Gate Size and Land Length
Size governs how long a gate stays open. DuPont’s Zytel guide sets gate thickness at 50 to 75 % of the part wall, at least 50 % for unreinforced nylon so that the part can be packed, and up to 75 % for glass-reinforced grades to limit fiber damage and to allow for their higher viscosity. The Delrin guide makes the same point in its own terms: a conical gate suited to amorphous resin lets acetal crystallize in the narrow tip before packing is complete, and the guide puts the loss of mechanical performance from poor packing at up to 30 %.
| Feature | Value | Source and condition |
|---|---|---|
| Gate thickness, nylon | 50 to 75 % of wall T, at least 50 % unreinforced | DuPont Zytel guide |
| Tunnel gate diameter, nylon | 0.5 to 0.6 T | DuPont Zytel guide, Figure 5.3 |
| Tunnel gate diameter, acetal | At least 0.5 T | Delrin molding guide |
| Tunnel diameter beside the gate | At least T + 1 mm (0.04 in) | Delrin guide and Zytel guide |
| Gate land, nylon and acetal | Under 0.8 mm (0.03 in), under 1 mm (0.04 in) in the Zytel text | DuPont Zytel and Delrin guides |
| Edge gate depth | 60 to 70 % of wall, width about twice the depth | Plastics Technology, common practice |
| Edge gate land | 0.51 to 1.14 mm (0.020 to 0.045 in) | Plastics Technology, general consensus |
| Pin gate diameter, PP | 1 to 1.5 mm (0.04 to 0.06 in), down to 0.7 mm (0.03 in) | Autodesk Moldflow PP page |
| Edge gate, PP | Depth at least half the wall, width at least twice the thickness | Autodesk Moldflow PP page |
| Runner feeding the gate | Not less than wall T (DuPont); about 1.5 T as a start (Plastics Technology) | DuPont Zytel guide; Plastics Technology |
The land is the short straight length between runner and cavity. Fattori writes that a longer land adds shear and lowers viscosity, which can help a long flow, but also adds pressure loss and can burn shear-sensitive resins. His advice is to start slightly long, because shortening a land is steel-safe, and to make every gate in a multi-cavity mold identical in depth, width and land length, or the cavities will not balance.
Tunnel gates need arithmetic. Fattori’s example is a 2.0 mm (0.080 in) wall with an edge gate 1.27 mm (0.050 in) deep and 2.54 mm (0.100 in) wide, a flow area of 3.2 mm² (0.0050 in²). A tunnel gate given the same 1.27 mm (0.050 in) “diameter” at 45° has an elliptical opening of only about 1.8 mm² (0.0028 in²), roughly half. For equal area, the minor diameter has to be about 1.70 mm (0.067 in). He adds that most complaints about tunnel gates freezing early or failing to pack come from gates that were simply undersized, and that tunnel gate orifices in a multi-cavity mold should agree within 0.025 to 0.05 mm (0.001 to 0.002 in) of each other, which is why he has them cut by EDM.
A gate is sized for packing, not for speed of freeze. A gate too small seals before the thick section is full, and a few hundredths of a millimeter between cavities make two different parts.
Gate Freeze and the Hold Time Study
The gate freeze test, or gate seal test, finds how long holding pressure has to stay on before the gate stops passing melt. Plastics Technology’s column by an RJG trainer sets out the procedure. Check cavity balance first and correct it if it is below about 95 %. Then mold parts at increasing hold times while keeping the total cycle constant, weigh them, and add hold time in steps of about 0.5 s for small parts and 1 to 2 s for larger ones.
John Bozzelli’s column on the same test asks for weights to four significant figures and a hold time long enough that the weight stops rising. DuPont’s Zytel guide describes the same study in steps of 0.5 to 1.0 s, with the runner and sprue removed before weighing, and notes that the method assumes the gate is correctly placed and sized.
| Curve shape | Example reading | Hold time set |
|---|---|---|
| Weight flattens, cold runner | Weight stable at 137 g from 5 to 6 s | 6.5 s for a frozen gate, 4.5 s to allow backflow |
| Weight keeps rising slowly, hot runner, valve gate or oversized gate | Weight rising about 0.5 % per extra second from 6 to 7 s | In the range where the increase is steady, read as stable after three steps under 0.5 % |
| Gate seal found, sealed gate preferred | Gate seal at 5.5 s | 6.5 s or more |
| Gate seal found, unsealed gate preferred | Gate seal at 5.5 s | Start at about half, 2.75 s, then tune pressure and time |
The freeze curve tells when the gate closes, not whether the gate is the right size. Fattori lists the signs that follow the test. A part still sinking, voided or undersized after the gate has frozen probably needs a deeper gate. A gate that takes a long time to freeze is probably too deep, unless the hold pressure is so high that semi-solid material keeps being pushed through. A large pressure loss or jetting at the gate points to a gate too shallow or a land too long.
Running With the Gate Sealed or Unsealed
Most molders are trained to hold until the gate seals. Bozzelli’s column questions the habit with a polypropylene rake that cracked at the gate on a cold morning. To fill the tines, the molder had set a high second-stage pressure and a long hold. The plastic near the gate froze packed tight while the far end, past the pressure drop along the flow, was packed less, and the dense gate region carried stresses that cold weather and raking added to.
His answer is a test, not a rule. Mold one set of parts with a hold time known to seal the gate and a second set with a hold time known to leave it open. Put both through the part’s performance tests across the full range of use temperatures. He reports that parts often fail on one side of gate seal and pass on the other, and that where performance is equal, the unsealed parts are lighter and use less resin.
The process steps that follow are in Table 2. For a sealed process, hold a little longer than the seal time, provided the screw can recover within the cooling time. For an unsealed process, start at about half the seal time and look for the center of the window that gives no sinks and in-specification dimensions.
Hot Runners, Valve Gates and the Dynamic Pressure Drop
A hot runner keeps the gate region molten, so the weight curve never quite flattens. Autodesk’s Moldflow help states the same thing for simulation: with injection into a hot runner, the injection location is held at the melt temperature and no gate cooling is applied, while a cold runner cools by the runner temperature calculation.
Plastics Technology’s column on hot runner and valve gate hold times, by Suhas Kulkarni, replaces the weight curve with a process window. On a two-cavity mold for an irrigation screen, parts were molded at hold pressures from 27.6 to 96.6 bar (400 to 1,400 psi) in steps of 13.8 bar (200 psi), at hold times from 4 to 10 s in 1 s steps. Sinks appeared at the low end and flash in the screen area at the high end. A designed experiment inside the cosmetic window then mapped one length, specified at 126.80 ±0.07 mm (4.992 ±0.003 in), for both cavities.
The combined window ran from 6.2 to 7.5 s at 43.5 to 63.5 bar (631 to 921 psi), and the process was set near its center, at 55 bar (798 psi) and 7 s. Kulkarni notes that on a molding machine pressure varies more than time, so the wider pressure range is the one to protect. The mold had needed one steel adjustment before that window existed.
Valve gates add a mechanical time. The RJG column notes that a pneumatic valve gate in good condition can take up to 0.2 s to close after the signal, and that the part loses weight during that interval. As the stems wear and stick, the closing time grows, and if it doubles to 0.4 s, the weight lost roughly doubles too. That is the reason to run the hold time study on a valve-gated tool as well: the hold time is set where the weight change is stable, so that wear shows up as a trend rather than a reject.
DuPont’s Zytel guide describes one more measure that reads the gate region from inside the cavity. With two pressure transducers, the dynamic pressure drop is the pressure at the first sensor when the melt reaches the second. Because it moves with melt viscosity, it shows a change in moisture or molecular weight while the press runs, before the change reaches the part as short fill or flash. DuPont’s chart for nylon 66 in a 2.0 mm (0.08 in) wall separates resin at 0.08, 0.15 and 0.22 % moisture.
On a hot runner or valve gate the gate never freezes in the cold-runner sense. The hold time is set from a measured window, and the valve’s closing time is watched as it wears.
What a Buyer Asks About the Gate
A gate is part of the tool and the drawing at once, and four questions settle it before steel is cut:
- Where is the gate, and where do the weld lines fall against the part’s loads and visible faces?
- What type and size of gate is planned, against the wall it feeds and the resin maker’s proportion?
- Was a hold time study run, and is the weight curve kept with the first article report?
- Will the process run with the gate sealed or unsealed, and was that choice tested on the part?
A gate can start small and be opened, because enlarging a gate removes steel, while shrinking one means welding. On a short-run tool that matters, since the first trial shows whether the thick sections pack before the gate seals. In low-volume injection molding for bridge production, the gate position is agreed on the part model and the hold time is taken from a weight curve at the first shots, so that the same gate makes the same part from the first lot to the last.
Sources and Further Reading
- Design rules of polymer injection locations, Moldflow 2014 help, Autodesk
- Number of polymer injection locations, Moldflow 2015 help, Autodesk
- Injection location temperature during packing and cooling, Moldflow 2015 help, Autodesk
- PP materials, Moldflow 2015 help, Autodesk
- Zytel and Minlon Nylon Resins Molding Guide, 2017, DuPont
- Delrin Technical Molding Tips, Technical Guide, 2024, Delrin
- Don’t Overlook Gate Location, Plastics Technology
- Injection Molding, Why and How to Do Gate-Seal Experiments, Plastics Technology
- Gate Freeze Study, Danger in a Name?, Plastics Technology
- Optimizing Pack and Hold Times for Hot-Runner and Valve-Gated Molds, Plastics Technology
- Tooling, How to Properly Size Gates, Runners and Sprues, Part 2, Plastics Technology
- Tooling, How to Properly Size Gates, Runners and Sprues, Part 3, Plastics Technology
- Tunnel Gates for Mold Designers, Part 1, Plastics Technology