GateDrawingAmorphous Resin

How Tightly Acetal Parts Hold Dimension in Injection Molding

Acetal dimension spread measured on one part under four press settings, with the gate and cooling rules behind it and a tolerance budget for a 50 mm feature.

Injection molded white acetal gears and clips with crisp teeth and smooth faces.

On one acetal test part, DuPont measured the outer diameter under four combinations of packing time and cooling time. The spread ran from plus or minus 0.02 mm in the best case to plus or minus 0.7 mm in the worst, a factor of 35 on the same resin, the same tool and the same machine. That best part also came off the machine in a 26 second cycle, against 41 seconds for the setting that gave plus or minus 0.07 mm.

Those four rows sit in the Delrin molding tips as a short table, and they answer the question a buyer asks before writing a tolerance on an acetal drawing: how tight can this resin be held, and what decides it. The answer is a mix of resin physics, gate geometry and two timers on the press.

Outer Diameter Spread Under Four Packing and Cooling Settings

The test part in DuPont’s tips is a tribological sample used for wear and friction testing, a part whose outer diameter has to be as dimensionally precise as possible. DuPont molded it under four settings, measured the outer diameter and reported the mean with its variation.

Table 1. Outer diameter of an acetal homopolymer test part under four settings, from DuPont’s Delrin molding tips
Trial Packing time Cooling time Cycle time Outer diameter, mean and variation
1 5 s 24 s 39 s 49.48 mm (1.948 in) ± 0.2 mm (± 0.008 in)
2 10 s 7 s 26 s 49.48 mm (1.948 in) ± 0.7 mm (± 0.028 in)
3 15 s 2 s 26 s 49.61 mm (1.953 in) ± 0.02 mm (± 0.0008 in)
4 15 s 15 s 41 s 49.76 mm (1.959 in) ± 0.07 mm (± 0.003 in)

The tips state that an optimum packing time of 15 seconds, the setting with the highest part weight, and the shortest cooling time resulted in the least warpage, and that similar results held for outer diameter. Trial 2’s variation is printed as 0.7 mm in the table, while the text refers to an increase in variability of 0.07 mm for the constrained trial 4, so the 0.7 should be read with the care a figure of that size on a 49.5 mm diameter deserves.

Three readings of the table stand out. In trial 1, short packing gave a small part, 49.48 mm, and a moderate spread. Trial 3, with full packing and almost no cooling in the mold, gave a larger mean, 49.61 mm, and the tightest spread by a wide margin. The fourth trial used the same full packing followed by a 15-second cooling in the mold, the way an amorphous resin is molded, and gave the largest part, 49.76 mm, and a spread three and a half times that of trial 3.

The mean size of an acetal part and the spread of its size are set by different settings. Packing time moves the mean. Cooling in the mold moves the spread.

The mean outer diameter moves by 0.28 mm between trial 1 and trial 4, which is 0.56 percent of the diameter. That is a movement of the size, separate from the variation within a trial, and it shows how far a process setting alone can shift a nominal dimension before any tolerance is applied.

Why Packing Fixes the Size and Mold Constraint Raises the Spread

Acetal homopolymer is one of the most crystalline of the semi-crystalline resins, at almost 60 percent crystalline according to DuPont, with a melt density of 1.17 g/cm³ against a solid density of 1.42 g/cm³ in the tips. Crystallization takes 11 percent of the volume, as the pressure-volume diagram in the tips shows, and cooling the solid takes a further 7 percent, which DuPont puts at about 2 percent in linear dimensions.

Packing replaces the first loss with new melt, and it can do so only while the gate is open. If packing ends early, as in trial 1, the part keeps the volume deficit, and it shrinks further, which fits the smaller diameter. Where packing runs to the end of crystallization, as in trial 3, the part leaves the mold full, and the remaining shrinkage is thermal.

The thermal stage is where the spread arises. DuPont states that the part should be allowed to shrink evenly and without constraint while cooling, and that this is best achieved by ejecting soon after pack-out and letting the part cool in air. A part kept inside the mold at that stage is held by the cavity walls and cores, and the constraint gives uneven shrinkage with visible and measurable warpage and deformation. The table shows the numeric version: constrained cooling in trial 4 raised the variation from 0.02 to 0.07 mm and the mean from 49.61 to 49.76 mm.

DuPont adds a point that matters for a part with ribs and bosses: if the thicknesses in a part differ and crystallization is compensated by an effective packing phase, the level of thermal shrinkage is independent of the thickness. The unevenness of an acetal part therefore comes mainly from packing and constraint, and much less from the wall steps themselves.

  • Short packing. A smaller part with more shrinkage and a moderate spread.
  • Full packing, ejected early. A larger part, tightest spread, shortest cycle.
  • Full packing, long cooling in the mold. The largest part and a wider spread, with constraint from the mold.

The table also shows what a buyer cannot read from it. It gives no wall thickness, no gate size and no mold temperature for the test part, so the exact numbers do not transfer to another part, and only the pattern does: pack to the plateau, eject early, cool in air.

Gate Geometry for a Part That Packs Fully

Packing is only as good as the gate that carries it. The DuPont tips contrast a tunnel gate with a conical gate and state that a conical gate, appropriate for amorphous resins, lets acetal crystallize in its narrow tip before packing is complete. Poor packing then means poor mechanical performance, by up to 30 percent, together with warpage and uncontrolled shrinkage. For the tunnel gate the tips give four criteria.

  • The gate sits in the thickest area of the part.
  • The gate diameter d is at least half the part thickness T.
  • The gate length is under 0.8 mm (0.03 in), so the gate does not freeze early.
  • The tunnel diameter D next to the gate is at least T plus 1 mm.

For a part of 4 mm wall at the gate, d is at least 2 mm, D is at least 5 mm and the gate land is shorter than 0.8 mm. Delrin’s molding guide adds a hold pressure of 60 to 110 MPa (8,700 to 16,000 psi), depending on the grade, and a hold pressure time of 8 s per mm based on a 3 mm wall, which on a 4 mm wall suggests 32 seconds as a first estimate. DuPont’s own test part found its optimum at 15 seconds, and the optimum is found by weighing parts, not by reading one figure off a sheet.

DuPont’s tips also supply a way to find the right packing time. The part weight is measured against packing time, and the optimum is where weight reaches its maximum. They add that the relationship between packing time and thickness is not linear, and that time per millimeter increases as thickness increases. A dimension controlled by weight is checked on the press by weighing, which a toolroom can do in a minute.

Ejecting Hot and Cooling Outside the Mold

The advice to eject hot is the least intuitive rule in the document for a molder trained on amorphous resins, where cooling in the mold sets the shape. For acetal, DuPont recommends ejecting the part from the cavity as soon as possible after pack-out and letting it cool slowly in air. It advises ejecting onto a conveyor before transferring into a bulk package, and it warns that ejecting straight into a box or bag creates a temperature gradient through the height of the container, which may give dimensional differences between parts at the top and the bottom.

The practical consequence for a dimension is a rule on handling. Parts from one run are cooled in the same way, laid out and not stacked hot, and measured after they reach the stated temperature. Delrin’s Design Guide Module III gives a thermal expansion of 0.91E-4 per K in the flow direction between 23 and 55 °C, so a 49.6 mm diameter that is 10 °C warmer at measurement reads about 0.05 mm larger than at 23 °C. A measurement of an acetal diameter at 33 °C is a measurement 0.05 mm away from the truth, and that is more than the 0.02 mm variation of trial 3.

The same mold also changes the cycle. Trial 3 and trial 2 both ran 26 seconds, and trial 4 ran 41 seconds, which makes the early ejection cycle 37 percent shorter than the constrained one, 26 against 41 seconds.

Annealing and Time After Molding

Delrin’s molding guide treats annealing as occasional, at 160 °C (320 °F) for 30 minutes plus 5 minutes per millimeter of wall, and it suggests annealing a part from a new mold as a test of how far post-molding shrinkage will go. Annealing is a stress-relief and stabilization step, and a part annealed for dimensional stability is measured after the step, not before.

For the 49.6 mm test part, with a wall of a few millimeters, the guide’s rule gives an annealing time of under an hour, and a part that hangs in an oven at 160 °C is held by its own geometry. DuPont’s nylon guide, written for a different resin, warns that complex parts may need lower annealing temperatures and times to limit deformation and recommends trials to find the conditions. The same caution applies to a thin or long acetal part.

A drawing that asks for an annealed dimension states the annealing conditions, the time between annealing and measurement, and the measurement temperature. Measured hot out of the oven, a part reads differently from the same part at 23 °C the next morning, and the two differ by the expansion at 1.0E-4 per °C, which on a 49.6 mm dimension is 0.005 mm per degree. Gauge rooms at 18 °C and 28 °C are 10 degrees apart, and that is 0.05 mm.

  • Before annealing. The dimension reflects the molding settings and the packing.
  • After annealing. The dimension reflects stress relief as well, and the drawing says which state counts.
  • At measurement. The part sits at the stated temperature long enough to be at it throughout.

A tolerance is a statement about a part in a state. The state is the packing, the cooling, the annealing and the gauge temperature, and each of them can move a 50 mm acetal dimension by hundredths of a millimeter.

A Tolerance Budget for a 50 mm Acetal Dimension

A direct tolerance is a budget with several items. The table sets the items known from the sheets for a dimension of about 50 mm, such as the outer diameter of the test part, and marks the ones that are not.

Table 2. Items in a tolerance on a 50 mm acetal dimension, with the number each source gives
Item Value for about 50 mm Source and condition
Process spread, best setting ± 0.02 mm (± 0.0008 in) DuPont test part, 15 s packing, 2 s cooling
Process spread, constrained cooling ± 0.07 mm (± 0.003 in) DuPont test part, 15 s packing, 15 s cooling
Process spread, poor setting ± 0.2 to ± 0.7 mm (± 0.008 to ± 0.028 in) DuPont test part, trials 1 and 2
Measurement temperature, 10 °C off 0.05 mm (0.002 in) Module III expansion of 0.91E-4 per K
Shrinkage allowance error, 0.1 point 0.05 mm (0.002 in) arithmetic on the data sheet’s 2.0 percent shrinkage
Moisture swell not stated Module III gives 0.2 % absorption at 50 % RH only
Tool wear at the gate not stated no shot count on the sheet or in the trade source

The first thing the budget says is that a plus or minus 0.05 mm tolerance on a 50 mm acetal dimension is within reach only for a well-set process. Trial 3’s spread of 0.02 mm leaves 0.03 mm for measurement temperature, allowance error and wear, and a setting like trial 4 uses 0.07 mm of spread before anything else counts.

The second thing is the list of items the sheets leave without a number. Moisture swell and tool wear are not quantified on the sheets, and a drawing that asks for a tight acetal tolerance has to agree them with the supplier, or leave margin.

Dimension Control on an Aluminum Bridge Tool

An aluminum tool changes three things about this picture. Its cavity temperature responds quickly to the cooling circuit, which the trade literature on aluminum tooling counts as an advantage in the process window. Gate and shutoffs are wear items in it, and the trade article from Plastics Technology advises checking for wear and galling every time the tool leaves the press, with coatings of about 5 to 8 µm raising surface hardness to 50 to 56 HRC where abrasive resins run. Acetal carries no glass, so abrasive wear is not the first concern, and a gate land that is 0.8 mm long at most is a feature whose wear shows in packing before it shows anywhere else.

DuPont’s best practices for dimension fit the order of work on a bridge tool.

  • Maintain the melt at the optimum temperature for stability, 215 °C with a tolerance of 5 °C for the standard grade.
  • Ensure the gate design meets the requirements of semi-crystalline materials.
  • Run the process with hold times adequate for maximum part weight.
  • Eject parts hot and let them cool outside the mold.
  • If dimensions miss the tolerance, check the gate design and the process conditions first.
  • If they still miss, correct the cavity.
  • Do not compromise process settings to achieve dimensional precision or consistency.

The order of the last three lines is the order of effort: a process setting takes minutes, a gate change takes hours and a cavity correction takes the tool out of the press. A buyer reviewing first samples can use the same order of questions, and ask for the check of part weight against packing time as evidence that the process was set before the cavity was touched.

Table 3. Items to write into an order for a tight acetal dimension
Item Wording
Grade Delrin 500P NC010, or the grade named in full
Measured feature the dimension, the temperature of measurement and the time after molding
Process evidence packing time on the weight plateau, cooling time stated, parts ejected hot and cooled in air
Gate tunnel gate within the four criteria, land length at most 0.8 mm
Sample first-article measurement of at least the critical dimension, signed before the run

An acetal dimension is held by packing the part fully, letting it cool without constraint and measuring it at a known temperature. For runs of a few to a few thousand parts, low-volume injection molding is the working form of bridge production.

Sources and Further Reading

Request an Injection Molding Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Injection Molding chosen.

Request a Quote