Aluminum Bridge ToolCavityPart Weight

How to Start Up an Injection Mold and Take the First Shots

A new mold is started cold on purpose, filled in stages with short shots, and read for vents, gates and heat before any process is fixed.

First shots from a new injection mold laid in a row, a short shot missing its end, a shot with flash, and a complete good part.

A nylon 66 melt has to read between 285 and 305 °C (545 to 580 °F) on a needle probe before the first part is any use, yet DuPont’s molding guide tells the setter to start the cylinder 10 °C below the low end of that range and then wait at least 20 minutes. The wait is the first lesson of a new mold. Heat soaks into a barrel from the outside, a screw that turns too early grinds unmelted pellets against steel, and a first shot taken on impatience tells you about the machine’s temperature, not about the tool.

A mold trial is a short, ordered set of moves with a reading at the end of each one. The sequence below follows that order for a thermoplastic going into an aluminum or soft steel bridge tool for the first time, using the start-up procedure and the fill, vent and gate figures that resin makers print in their own molding guides. Where a figure belongs to one resin, the resin is named.

The Start-Up Sequence from a Cold Barrel to the First Shot

Eight moves take a machine from cold to its first complete part. The first four prepare the melt, the next three shape the shot, and the last one is a decision: whether the part describes the tool or only the settings.

DuPont’s guide for Zytel and Minlon nylons gives the melt side of this in plain steps. The machine starts clean and purged, with the hopper inlet shut. Cylinder zones go 10 °C (20 °F) under the lowest melt temperature the maker recommends, the nozzle goes to its working temperature, and a cold machine gets at least 20 minutes for the heat to work in before the zones are raised to operating levels.

The remaining steps check what the heaters cannot promise. Jog the screw, and if it will not turn, give it longer to soak. If it still will not turn after a longer soak, a higher-melting resin from the last job may not have left the barrel.

Once the screw turns, open the hopper inlet briefly so some resin covers it, close it, rotate the screw and read the drive torque. Excessive torque points to a rear zone that is too cool.

The first reading of a trial is the melt, not the part. A needle-probe temperature taken from an air shot shows whether the next hour of results can be trusted.

Only then does the injection cylinder move forward against the mold. The same guide recommends repeating the probe check whenever a significant change to the cycle is made, because a longer or shorter cycle changes how long the melt sits in the barrel and so how hot it is when it arrives.

Table 1. Start-up sequence for a thermoplastic going into a new mold, with the figure each step runs on
Step Move Reading or setting Source
1 Purge the barrel and close the hopper inlet Clean barrel before heating DuPont Zytel and Minlon molding guide
2 Heat the cylinder below target 10 °C (20 °F) under the minimum melt temperature; nozzle at processing temperature DuPont Zytel and Minlon molding guide
3 Soak a cold machine At least 20 min; at least 30 min at about 20 °C (35 °F) under the melting point for a hot runner DuPont Zytel and Minlon molding guide
4 Jog the screw and open the hopper briefly Screw turns; torque checked DuPont Zytel and Minlon molding guide
5 Probe the melt on an air shot Needle pyrometer reading inside the resin maker’s range DuPont Zytel and Minlon molding guide
6 Bring the unit forward with a short shot Transfer position set to give a short shot and no pack pressure DuPont Zytel and Minlon molding guide
7 Move the transfer point later until the cavity fills As late as possible, never after the mold is full DuPont Zytel and Minlon molding guide
8 Adjust for appearance, then maximum part weight Pack time then fixed by a weight study DuPont Zytel and Minlon molding guide

Heat Soak, Hot Runners and the Barrel Between Shots

The soak is not only for the barrel. A hot runner manifold and its nozzles are metal masses that heat from the heaters inward, and the same guide asks for the manifold to be brought to about 20 °C (35 °F) below the resin’s melting point and held at least 30 minutes before the final heat-up. Modern controllers can run that stepwise start automatically.

A bridge tool in aluminum raises a separate point. Arconic’s fact sheet for QC-10 aluminum states that hot runner systems can be integrated successfully into aluminum molds, but the mold and hot runner design have to account for aluminum’s thermal and mechanical properties. Aluminum conducts heat 4 to 5 times better than P-20 steel, so the sheet calls for thermal isolation of the manifold, with a water-cooled hot half plate as the simplest method.

The sheet also puts QC-10’s expansion at twice P-20’s, 24.7 × 10⁻⁶ per K (13.7 × 10⁻⁶ per °F) against 12.2 × 10⁻⁶ per K (6.8 × 10⁻⁶ per °F) in thyssenkrupp’s table, and asks designers to allow for it. At first heat-up the manifold and the tool grow by different amounts, which is one more reason to allow the full soak.

If dead spots in a hot runner are suspected, DuPont proposes a color change in the cylinder and a further 10 minutes of molding without a break. The system is then shut down and taken apart to find the places that still hold the first color. Those places are where degraded resin will later be released into good parts.

Resin choice sets how forgiving the barrel is. DuPont states that its Delrin acetal homopolymer stays stable for over 30 minutes at the recommended 215 ± 5 °C melt (419 ± 9 °F), and it asks for the machine nozzle or hot runner at 190 °C (374 °F). If those have to be set higher for other reasons, degradation can begin after a few hours of running and cleaning gets more frequent. A resin that tolerates less time at temperature makes a long mold trial, with stops for measuring and adjusting, a degradation risk in its own right.

Finding the Transfer Point With Short Shots

Filling the cavity in stages shows how the tool fills. The usual way in is to set the transfer position, the screw position where the machine switches from speed control to pressure control, so early that the part is visibly incomplete. DuPont’s start-up step says the same: the first transfer position is chosen to leave a short shot with no pack pressure, unless an incomplete part would make ejection unsafe.

Each step later in the transfer position adds more of the cavity. Short shots, lightly ejected and laid out in a row, show the flow front in order. They show which end of the cavity fills last, which weld lines will form where fronts meet, and where gas will be trapped. A setter who skips this and starts with a full, packed part loses the picture that explains the weld line and the burn mark that appear later.

The same guide gives the target: switch from the speed-controlled injection phase to the pressure-controlled hold phase as late as the process allows, yet never after the cavity is full. Going earlier leaves the hold phase to finish the filling at low speed. A later switch drives pressure into a full cavity at injection speed, and the guide warns of a stressed zone near the gate and weaker parts.

Take the transfer point later one step at a time until the cavity just fills at the end of the speed phase. That is the setting the pack phase then builds on.

A semi-crystalline resin and an amorphous one ask for different things afterward. In the Delrin tips sheet, a bad process with an amorphous resin tends to over-pack the part, while with a semi-crystalline resin it tends to under-pack and shrink too much. That difference sets how aggressive the later pack settings are, and the first shots show which side the tool leans toward.

Fill Speed, Fill Time and the Burn Mark at the End of Flow

Fill speed is chosen against how fast the resin freezes. DuPont’s nylon guide calls 1 to 3 seconds a fast fill, wanted in thin sections, and prefers slower fills for thick ones. Glass-reinforced and other nucleated nylons freeze sooner than unreinforced grades and need fast fills, but an injection speed that is too high overshears the melt at the gate and costs properties. A chart in the guide relates the maximum fill rate to round gate diameter for unreinforced nylon 66, which makes the gate a limit on fill speed.

A poor surface from a slow fill is a common false reading. The guide traces frosting to melt that starts to solidify before the cavity is full, and says it is often taken for bad fiber dispersion or for wet resin. Chasing the wrong cause wastes a day, so change fill speed alone and look at the surface before touching the dryer or the screw.

At the end of the flow path, air has to leave the cavity before the resin arrives. For burning at the end of flow the guide proposes a two-stage fill, fast through most of the cavity and slower near the end. A slower last stage gives the vents more time, but it does not replace vents.

Table 2. Vent and gate dimensions that DuPont gives for nylon resins, converted for tool review
Feature Dimension In inches Source note
Vent depth, Zytel and Minlon PA 0.012 to 0.020 mm 0.0005 to 0.0008 in Min to max from the vent table
Vent land length 0.8 to 1.0 mm maximum 0.03 to 0.04 in Land should not exceed 0.8 mm in the text
Vent width As wide as feasible, typically over 3 mm Over 0.12 in Vent area is width times depth
Relief channel depth Over 0.8 mm, opened to about 3 mm after 25 mm Over 0.03 in, then 0.12 in after 1.0 in From the venting figure
Gate thickness 50 to 75 % of part thickness Not applicable Gate design summary
Gate land length Under 1 mm Under 0.04 in Prevents premature solidification
Draft per side 0.5° to 1° Not applicable Softer, more elastic resins up to 2°
Undercut in glass-reinforced nylon Avoid over 3 % Not applicable Low elongation of glass-reinforced grades

Venting and Gate Size Read From the First Parts

The first parts are the earliest honest review of the tool.

DuPont’s guide ties weak venting to a list of faults: weak weld lines, burned or discolored spots, attack on the steel, size variation, bubbles or blisters on the surface, and short shots. Cavities and runners are vented at the parting line and at the ejectors. The land stays at or under 0.8 mm (0.03 in), and the passage behind it widens with distance from the cavity edge. For low-viscosity grades where flash has to stay minimal, vents can be sized conservatively shallow and deepened as required, which suits a bridge tool, because it is easier to cut a vent deeper than to weld it back.

Gate design shows in the packing behavior, which the first shots only hint at. The guide gives gate thickness at 50 to 75 % of part thickness and a land length under 1 mm, since a longer land freezes the gate before the part is packed. Delrin’s sheet is firmer for a highly crystalline resin: the tunnel gate diameter at least half the part thickness, a gate length under 0.8 mm, and the tunnel diameter next to the gate at least the part thickness plus 1 mm. A conical gate suits amorphous resins, but Delrin crystallizes in a narrow tip before packing is done, which DuPont links to up to 30 % loss of mechanical performance, warpage and uncontrolled shrinkage.

An aluminum bridge tool can be changed after the first shots in ways a hardened steel tool cannot. Aluminum machines easily and can be cut deeper at a vent or enlarged at a gate. This is the practical edge of bridge tooling, and the first shots are the point at which that edge is used. You decide which changes go back to the toolmaker and which stay as process settings.

Reading the First Parts for Faults

Each fault on a first part points at a limited set of causes, and the order in which you check them matters. Start with the process changes that cost nothing, then the material, then the tool.

  • A short shot with a smooth, rounded flow front usually means the transfer is too early or the fill speed too low for the section, while one with a burned edge points to trapped gas.
  • Silver streaks or splay point first to moisture in the resin, and then to melt that is too hot or too long in the barrel.
  • Frosted surfaces on a glass-reinforced part indicate that the cavity wall is too cold or the fill too slow, and DuPont’s guide puts reinforced nylons near 100 °C (210 °F) in the mold for a better surface and less frosting.
  • Flash at the parting line shows excess pressure, a worn or contaminated shut-off, or a vent that is too deep.

A part that sticks in the mold tells its own story. Covestro’s processing sheet for Makrolon TC polycarbonate notes that a mold temperature that is too high can cause slight delamination and residue in the mold, and suggests 65 to 82 °C (150 to 180 °F) to avoid sticking within a wider 65 to 100 °C (150 to 212 °F) range. It also names beryllium copper for ribs, deep cores and other spots prone to sticking, and different temperatures on the two halves to hold the part on the intended side. Many of these parts had a forerunner: the same design made as vacuum cast copies or as 3D printed parts while the tool was built, and the first shots are where the molded part is first compared with what those copies showed.

Table 3. First-shot faults, the first thing to change and the second
What the part shows Change first Check second
Short shot, smooth front Transfer point later or fill speed higher Melt temperature on the probe
Burn mark at the end of flow Slower last stage of fill Vent depth and land at that spot
Frosting on a glass-filled part Faster fill, hotter mold Gate size
Splay Resin dryness Melt temperature and hold-up time
Part stays on the wrong half Mold half temperatures Draft and ejector position
Flash at the parting line Pack or hold pressure Shut-off condition and vent depth

Interruptions, Purging and Closing the Trial

Mold trials stop often, to measure, to cut steel and to wait for a decision. For a short stop DuPont recommends pulling the injection unit back, lowering the cylinder settings until the melt sits 30 °C (60 °F) under the recommended value, and firing frequent air shots to clear resin that is starting to degrade. A long stop calls for a purge with high density polyethylene or polystyrene.

The purge choice is not trivial. DuPont’s picks are polystyrene, cast acrylic (nozzle removed) and high density polyethylene, which stay stable over a wide temperature range and leave other polymers alone. The procedure pulls the unit back, runs the screw fast to pump out the old resin, feeds purge resin until the output is clean, and finishes with several fast air shots that scrub the cylinder walls.

Covestro adds a warning from its own polycarbonate. Makrolon TC is viscous and runs hot, so it can lift deposits left by the previous material, which is why it asks for purging before production. Its sheet pictures a screw, nozzle and check ring after about an hour of standing in the barrel at molding temperature, a condition that can stop the screw and send it to be pulled and cleaned by hand. A trial that pauses for an hour at full temperature can cost more time than the trial itself.

Never leave a barrel hot and full during a long pause. Drop the melt temperature and take air shots on a short stop, and purge for a long one.

Shutdown follows the same logic: close the hopper inlet while continuing to cycle, empty the barrel, add purge resin until the output is clean, leave the screw forward and switch off the power. The result is a clean start the next day, with one less variable in the next trial.

What the First Shots Hand to the Next Step

By the end of the trial three records should exist.

  1. The melt temperature and the dwell behind it.
  2. The transfer position and fill time that just fill the cavity.
  3. A list of tool changes, with the shot number at which each was found.

Those records feed the pack and hold study, where the part weight is plotted against the pack time to find the point at which the gate freezes, and the first article inspection, where dimensions are read against the drawing.

The record has a second use for a bridge program. A soft steel or aluminum tool is cut once and corrected a few times, and a buyer approving samples will want to know which corrections were made to the tool and which to the process. Keep the settings sheet and carry it into production, because it lets the same part be repeated on another press without rediscovering the process from scratch. For anyone sending a drawing to a toolmaker, low-volume injection molding is where this order of work begins, and bridge production is where its records are used again.

Sources and Further Reading

Request an Injection Molding Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Injection Molding chosen.

Request a Quote