DuPont’s molding guide for nylon gives a vent depth of 0.012 to 0.020 mm (0.0005 to 0.0008 in) at the parting line. Below that gap the air in the cavity cannot leave fast enough and the part may stop short of the last corner. Above it the melt follows the air out and leaves a fin. The whole difference between an unfilled part and a flashed one can sit in eight thousandths of a millimeter of ground steel.
Short shots, sink marks and flash are the three defects a buyer sees first on a sample tray, and they are linked. Each one is a mismatch between the volume of melt the press delivers, the pressure that pushes it, and the space the mold allows it. This piece traces each defect to the causes the resin makers list, shows why fixing one so often produces another, and sets out the checks that tell a molder which cause is at work before a setting is touched.
What Short Shots, Sink and Flash Have in Common
A short shot is a part the cavity never finished. BASF’s troubleshooting brochure for engineering thermoplastics describes it as a part not completely formed, mainly in the areas furthest from the gate or in thin walls. A sink mark is an indentation where the wall thickens, because the volume lost as the thick section cools was not made up by holding pressure. Flash is a thin fin of excess material that forms where the melt has pushed into gaps and joints in the parting surfaces.
Read side by side, the three share one axis. Too little melt, too little pressure or too little time gives a short shot or a sink. Too much pressure for the clamp, or a melt runny enough to enter a gap the tool should have sealed, gives flash. Venting sits on the same axis from the other side, because a vent deep enough to let all the air out is also a gap the melt can follow.
| Defect | Cause listed | Remedy listed |
|---|---|---|
| Short shot | Not enough melt metered in | Increase the metering stroke |
| Short shot | No melt cushion | Check the non-return valve |
| Short shot | Melt or mold temperature too low | Raise melt temperature first, then mold temperature |
| Short shot | Mold not adequately vented | Check and improve the vents |
| Short shot | Wall too thin or flow path too long | Thicken the wall, move or add gates, add a flow leader |
| Sink mark | Holding pressure does not make up the cooling contraction | Raise holding pressure and hold time, set by part weight |
| Sink mark | Sudden change in wall thickness | Ribs at half the wall thickness, even walls along each flow path |
| Sink mark | Part gated into a thin wall | Gate where the wall section is greatest |
| Flash | Clamping force too low | Raise clamp force or use a larger machine |
| Flash | Fit of mold halves or splits too loose, sealing faces damaged | Correct the fits, repair the parting surface |
| Flash | Cavity pressure too high in fill and hold | Earlier change-over, slower injection at the end of fill |
| Flash | Melt viscosity too low from heat, long residence or moisture | Lower melt temperature, cut residence time, dry the resin |
Two rows in that table point in opposite directions. Raising melt temperature is a remedy for a short shot, and lowering it is a remedy for flash. That is the first sign that the defects cannot be cured one setting at a time.
Short shot, sink and flash are three readings of one balance between melt volume, pressure and the space the steel allows. A remedy for one is often a cause of another.
Short Shots and the Causes Behind an Unfilled Cavity
The first question on a short shot is whether enough melt reached the cavity at all. BASF lists a metering stroke that is too short and a missing melt cushion as the first two causes. The cushion is the melt left in front of the screw after the pack and hold phase, and Plastics Technology’s account of it by Suhas Kulkarni explains why it matters: with no melt in front of the screw, no force on the screw reaches the cavity, so the part is short or underpacked.
Kulkarni gives a working figure. For screw diameters of 25 to 60 mm (1.0 to 2.4 in), the cushion is held around 5 mm (0.20 in), with alarm limits typically about ±1.3 mm (0.05 in) set from the part’s own dimensional tolerances. A cushion that drifts toward zero is a short shot about to happen. A cushion that is too large consumes pressure compressing the melt and can feed degraded material from the hot nozzle zone into the part.
A cushion that disappears on a press that ran well an hour ago points to the non-return valve. BASF lists a check of its sealing function under short shots, sinks and voids alike. A valve that does not close lets melt flow back along the screw during injection, so the stroke looks right and the cavity still receives less.
When the melt is all there and the cavity is still short, the causes move to the mold and the material:
- Temperature. BASF advises raising melt temperature before mold temperature, because a hotter melt lowers the filling pressure, while a hotter mold also lengthens cooling.
- Injection speed. A speed too low lets the flow front freeze before the far end fills.
- Venting. Trapped air at the end of fill compresses and stops the melt, and may also burn it.
- Pressure loss in the feed. A narrow nozzle, runner or gate spends pressure before the melt reaches the part.
- Geometry. A wall too thin for the flow length, or a thin section near the gate that freezes during fill, leaves the rest of the cavity starved.
The last cause is the one a buyer can see on the drawing. BASF’s remedy is to move the gate so that the thin area fills last, or to add a runner, and to choose a material that flows more easily if the process has already been optimized and the part still does not fill.
Sink Marks and Voids Where the Wall Thickens
A sink mark is a short shot of a different kind: the cavity filled, but it was not packed. BASF explains that the thick section shrinks more in volume as it cools, and the shrinkage pulls the surface layer inward. Some sinks appear only after ejection, when the hot core reheats the skin and lets it yield. Others show only as a change in gloss.
A void is the same shrinkage turned inward. When the skin has already frozen too stiff to follow the contraction, the material pulls apart in the middle of the wall and leaves bubbles or microcells. BASF gives a simple way to tell a void from a gas bubble: drill into the part while holding it under water, and water entering the hole shows a void.
The process remedy is holding pressure and holding time, and BASF sets out how to find the time. Start with a short hold, raise it in steps, and weigh the part or watch cavity pressure until no further change appears. That point is the gate open time, and the hold is set somewhat longer. DuPont’s nylon guide describes the same weighing study in steps of 0.5 to 1.0 s, with the runner and sprue removed before weighing.
The design remedy is wall thickness. BASF’s brochure recommends ribs at half the wall thickness, no sudden changes of section and no thin sections along a flow path. A rib or boss makes a locally thick region that cools more slowly than the wall beside it, and Plastics Technology’s report on sink reduction names that differential cooling as the source of the depression.
That report, by a SABIC engineer on a study run at GE’s Polymer Process Development Center, compared eight tooling methods against a plain steel boss pin. Its test plaque had a nominal wall of 2.5 mm (0.100 in) and a boss 22.25 mm (0.875 in) high and 4.5 mm (0.177 in) in diameter, with a boss wall of 1.90 mm (0.075 in) and gussets 2 mm (0.079 in) at the base. Parts were deliberately underpacked so that sink could be measured on a coordinate measuring machine rather than judged by eye.
| Method | Kind | PC/ABS outcome | PPE/PS outcome |
|---|---|---|---|
| Spring-loaded boss pin | Material displacement | Better than baseline, up to 50 % less sink when tuned | Better than baseline, up to 50 % less sink when tuned |
| Protruding boss pin, 25 % and 50 % into wall | Material displacement | Poor | Better than baseline |
| Radiused boss pin | Material displacement | Poor | Poor |
| Gas assist through the pin | Material displacement | Inconclusive, melt froze too fast in thin walls | Better than baseline |
| Chemical foaming, 0.25 % blowing agent | Material displacement | Inconclusive, splay seen | Not better than baseline |
| Beryllium copper boss pin | Heat removal | Better than baseline | Better than baseline |
| Beryllium copper insert | Heat removal | Better than baseline | Not better than baseline |
| Active thermal boss pin | Heat removal | Better than baseline | Not better than baseline |
The study’s surprise was the protruding pin, recommended for about two decades, which did poorly in PC/ABS. Its authors found that spring preload mattered more than spring stiffness: too little preload let the melt push the pin back and add material, too much made it behave like a plain pin.
A sink is an unpacked section, and the cure starts with a hold time found by weighing parts. Where the geometry still sinks, a change at the boss pin can halve it, but which change works depends on the resin.
Flash at the Parting Line and the Vents
Flash has two common sources, according to Plastics Technology’s column on the flash-and-shorts chase by Garrett Gattshall: cavity pressure that exceeds the clamp force, and mold damage. Once cavity pressure overcomes the clamp, the mold opens a little and melt escapes. A damaged parting line lets it escape even when the clamp holds. A blocked gate can cause the first case on its own, because the cavities still open receive the pressure meant for all of them.
BASF adds the material side. A melt that is too hot, held too long in the barrel or hot runner, or processed wet, loses viscosity and enters gaps a normal melt would bridge. Drying the resin and shortening residence time are therefore flash remedies as much as remedies for splay.
Vents are the gaps the mold maker cuts on purpose. A vent has a depth, a land length across which that depth is held, and a relief channel behind it that carries the air away. Resin makers set the depth by how runny the melt is.
| Dimension | Value | Source and condition |
|---|---|---|
| Vent depth, nylon (Zytel and Minlon) | 0.012 to 0.020 mm (0.0005 to 0.0008 in) | DuPont, minimum to maximum |
| Vent depth, runny crystalline resins such as nylon, PE, PP | 0.013 to 0.025 mm (0.0005 to 0.0010 in) | Plastics Technology, typical maker range |
| Vent depth, viscous amorphous resins such as PC, TPU, PEEK | 0.025 to 0.076 mm (0.0010 to 0.0030 in) | Plastics Technology, typical maker range |
| Vent land length | 0.8 to 1.0 mm (0.03 to 0.04 in) maximum | DuPont |
| Vent land length | 0.76 mm (0.030 in) minimum by consensus, a start at 2.0 mm (0.080 in) on large parts | Plastics Technology |
| Vent width | Typically over 3 mm (0.12 in), as wide as feasible | DuPont |
| Vent width | 6.4 mm (1/4 in) on small parts, 12.7 mm (1/2 in) on larger | Plastics Technology, standard grinding wheel widths |
| Relief channel depth | Over 0.8 mm (0.03 in), opened to about 3 mm (0.12 in) after 25 mm (1.0 in) | DuPont |
| Primary relief channel depth | At least 10 times vent depth, minimum 0.51 mm (0.020 in) | Plastics Technology, author’s rule |
The column, by Jim Fattori, adds a point that matters for flash. A vent flashes only if it is too deep, never because it is too wide. Wall thickness also changes the safe depth: a test mold with 18 tabs of different thickness showed that thicker walls tolerate deeper vents, because a thin section raises the shear rate, lowers viscosity and raises the pressure at the end of fill. Near a gate or at the base of a thin rib, the shallow end of the range is safer.
Vents also wear and clog. Fattori notes that polished vents extend the maintenance interval but still gather sticky residue over a few thousand to tens of thousands of cycles. A vent that has filled with residue is a short shot waiting for its cause, and a vent ground deeper to cure it is flash waiting for its cause.
Why Correcting One Defect Brings Back Another
Gattshall’s column gives the clearest account of the chase. Shorts appear, so the vents are deepened. Flash follows, so the melt temperature is lowered to raise viscosity. Injection pressure climbs until the process is pressure limited, and sporadic shorts return.
The same loop runs on hold pressure. A technician who raises hold pressure to clear a short, without finding why the short appeared, can create flash once the sporadic cause goes away. Gattshall’s example is debris lodged in the non-return valve: while it holds the valve open, a larger shot hides the problem, and once it works free, the extra shot flashes the mold.
His conclusion is a rule for process development. At the optimal process setting, decide which defect is really present. If flash prevents the hold pressure from being raised high enough to absorb normal variation, the problem to solve is the flash, even if the parts on the bench today are short.
When a press that made good parts starts making short or flashed ones, something in the process changed. A setting moved in reaction to the defect hides the change and starts the chase.
Reading the Melt With Dynamic Pressure Drop
Several causes in Table 1 come down to melt viscosity: temperature, residence time, moisture, degradation. DuPont’s Zytel guide describes a way to watch viscosity during production instead of guessing at it. Two pressure transducers sit in the cavity, and the dynamic pressure drop is the pressure at the first sensor at the moment the melt reaches the second.
When the melt thins, the pressure needed to push it from one sensor to the next falls. DuPont’s chart for nylon 66 in a 2.0 mm (0.08 in) wall plots this pressure drop against relative viscosity for resin at 0.08, 0.15 and 0.22 % moisture. The guide names the reason the reading moves: hydrolysis and polycondensation during processing change molecular weight, and moisture, melt temperature and hold-up time all act on those reactions at once.
For flash, that link is direct. A wet or overheated nylon melt has the low viscosity BASF lists as a flash cause, and the pressure drop between two sensors shows the change on every shot. The same guide gives the hold pressure DuPont uses for nylon, usually around 90 MPa (13,000 psi), and notes that a change of 10 MPa (1,450 psi) moves shrinkage by about 0.1 %, which is a measure of how much a sink depends on the pressure setting.
The guide also warns against splitting the hold into several pressure levels on a semi-crystalline resin. One pressure over the whole hold time gives uniform crystallinity, and the hold is set so that the gate freezes when the part has crystallized, not before.
Tracing a Defect From the Part Back to Its Cause
DuPont’s troubleshooting table for Zytel sets out remedies for 13 problems, short shots, sinks, voids and flashing among them, in a suggested order for each. The guide’s own advice on the order is practical: test the sensitivity of a process setting such as pack time before a slower and more costly change such as gate size. A molder who follows that order changes steel last.
Plastics Technology’s column on fill time adds a method that shows where a cavity fills last. In a short-shot progression, the transfer position is stepped so that partly filled parts show the flow front at each stage. Gattshall’s team found that a faster fill improved fill balance only up to a point, after which air could not vent fast enough and burns appeared at the end of fill. The slower fill with the best balance ran with fill time varying by about 0.02 s.
For a buyer receiving first samples with any of the three defects, these are the questions that separate a traced cause from a moved setting:
- Was a short-shot progression run, and where does the part fill last?
- What is the cushion, and is it alarmed on the press?
- How was hold time set, and is there a part weight curve behind it?
- Was the resin dried to the maker’s moisture limit, and is a moisture or pressure record kept by lot?
- Are the vents at the end of fill, and at what depth for this resin?
- If flash appeared, was the parting line inspected for damage before clamp force or pressure was changed?
Answers to those six turn a sample tray into evidence. A short part with a logged cushion of zero tells a different story from a short part with a full cushion and a clogged vent, and the remedy follows from the story.
The defect on the part is a symptom. The cushion, the part weight curve, the vent depth and the resin moisture are where the cause is found.
Steel changes are the slow end of the list, and on a new tool they are cheapest before the tool is hardened or coated. Vents can be cut to the shallow end of the resin’s range and opened in steps, gates can start small and grow, and a boss that sinks can be tried with a different pin before the wall is redesigned. In low-volume injection molding for bridge production, a short-shot study and a part weight curve taken at the first trial keep these three defects from following the tool into the run.
Sources and Further Reading
- Injection-Molding Problems in Engineering Thermoplastics, Causes and Solutions, BASF
- Zytel and Minlon Nylon Resins Molding Guide, 2017, DuPont
- Don’t Get Caught in the Flash-and-Shorts Chase, Plastics Technology
- How to Reduce Sinks in Injection Molding, Plastics Technology
- Consider the Cushion When Seeking Shot-to-Shot Consistency, Plastics Technology
- Back to Basics on Mold Venting, Part 2, Shape, Dimensions, Details, Plastics Technology
- Is Faster Always Better When It Comes to Injection Molding Fill Times?, Plastics Technology