Polycarbonate Injection Molding Properties for Clear and Tough Parts

Polycarbonate read from the maker's sheets for a buyer: what it molds like when dry and hot, how thin walls fill, and what to ask of an aluminum tool.

Injection molded clear polycarbonate parts, a lens cover, a housing and a light guide, glass clear.

Covestro’s Makrolon 2407 data sheet gives its barrel zones as 250 to 270 °C at the rear, 270 to 290 °C in the middle and 285 to 305 °C at the front, with a standard melt of 300 °C (572 °F). The resin that leaves that barrel is transparent, passes 89 percent of visible light through a 2 mm wall and takes a steel-like punch from a puncture test. It also asks for drying at 120 °C (248 °F) for 4 hours before it goes in, down to 0.02 percent moisture.

Those three facts, a hot melt, a wet-sensitive pellet and a clear tough part, set most of what a buyer needs to know about polycarbonate in injection molding. The sections below read the maker’s published data for one general-purpose grade, then show where thin walls, thermally conductive grades and aluminum tooling change the picture.

Makrolon 2407 Properties in Metric and Inch Units

Makrolon 2407 is a low-viscosity, general-purpose, UV-stabilized, easy-release polycarbonate with a melt volume-flow rate of 19 cm³/10 min at 300 °C and 1.2 kg under ISO 1133. Its ISO short name is ISO 7391-PC,MLR,(,,)-18-9. The datasheet used here is the ISO edition dated 30 November 2017, and its values are typical, not guaranteed.

Table 1. Makrolon 2407 properties at 23 °C and 50 percent relative humidity unless stated, from Covestro’s ISO datasheet
Property Value Inch or US unit Test
Density 1,200 kg/m³ 0.0434 lb/in³ ISO 1183-1
Tensile modulus 2,400 MPa 348,000 psi ISO 527-1, -2
Yield stress 66 MPa 9,600 psi ISO 527-1, -2
Strain at break 120 % 120 % ISO 527-1, -2
Flexural modulus 2,350 MPa 341,000 psi ISO 178
Flexural strength 98 MPa 14,200 psi ISO 178
Charpy notched impact, 3 mm, 23 °C 65 kJ/m², partial break 31 ft·lb/in² ISO 179-1eA
Charpy notched impact, 3 mm, -30 °C 14 kJ/m², complete break 6.7 ft·lb/in² ISO 179-1eA
Puncture energy, 23 °C 55 J 41 ft·lb ISO 6603-2
Glass transition temperature 143 °C 289 °F ISO 11357-1, -2
Heat deflection at 1.80 MPa 124 °C 255 °F ISO 75-1, -2
Heat deflection at 0.45 MPa 136 °C 277 °F ISO 75-1, -2
Linear thermal expansion, 23 to 55 °C 0.65E-4 per K 3.6E-5 per °F ISO 11359-1, -2
Water absorption, equilibrium at 23 °C and 50 % RH 0.12 % 0.12 % ISO 62
Water absorption, saturation in water at 23 °C 0.30 % 0.30 % ISO 62

Two entries need a second look. The notched impact figure falls from 65 kJ/m² to 14 kJ/m² between 23 °C and -30 °C, and the break changes from partial to complete over that span. A bracket that is tough in the workshop can snap in a cold chain, so the notch radius and the cold-impact condition belong in the specification of any polycarbonate part that sees frost.

The ball indentation hardness is 116 N/mm² under ISO 2039-1, and the resistance to heat under the ball pressure test is 135 °C under IEC 60695-10-2. Heat deflection is reported unannealed on a bar, so a part with molded-in stress can soften sooner than the bar does.

The sheet’s temperature figures describe a polymer with a glass transition at 143 °C. Below that point the part is a glassy solid, above it the part flows, and a clear housing near a heat source is judged by its stress and its geometry, not by the sheet’s headline number.

Clarity numbers for transparent parts

The same sheet lists luminous transmittance for clear material at 89 percent at 1 mm and 2 mm, 88 percent at 3 mm and 87 percent at 4 mm under ISO 13468-2, with haze below 0.8 percent at 3 mm under ISO 14782 and a refractive index of 1.584. Thicker walls lose about one point of transmittance per millimeter beyond 2 mm, so a clear window drawn at 4 mm loses two points against a 2 mm window before any surface effect enters.

Drying, Melt and Mold Temperature for Polycarbonate

Polycarbonate carries 0.12 percent water at equilibrium in room air, and the sheet sets a ceiling of 0.02 percent moisture in the pellet at the press. Its recommendation is dry-air drying at 120 °C for 4 hours. Covestro’s processing sheet for thermally conductive grades repeats the principle with a desiccant dryer at 121 °C (250 °F) with an inlet dew point of -29 °C (-20 °F), a minimum of 4 hours and a moisture content below 0.02 percent.

Table 2. Recommended processing conditions for Makrolon 2407, from the same datasheet
Setting Range Inch or US unit
Melt temperature 280 to 320 °C, standard 300 °C 536 to 608 °F, standard 572 °F
Barrel, rear 250 to 270 °C 482 to 518 °F
Barrel, middle 270 to 290 °C 518 to 554 °F
Barrel, front 280 to 290 °C 536 to 554 °F
Barrel, nozzle 270 to 305 °C 518 to 581 °F
Mold temperature 80 to 120 °C 176 to 248 °F
Hold pressure 50 to 75 % of injection pressure 50 to 75 %
Plastic back pressure 100 to 200 bar 1,450 to 2,900 psi
Peripheral screw speed 0.05 to 0.2 m/s 2 to 8 in/s
Shot size to cylinder 30 to 70 % 30 to 70 %
Vent depth 0.025 to 0.075 mm 0.001 to 0.003 in

The test specimens behind the properties in Table 1 were molded at a melt of 280 °C, a mold at 80 °C and an injection velocity of 200 mm/s, the conditions the sheet attaches to ISO 294. A part molded at 300 °C and 100 °C in the tool is not that specimen, and its shrinkage, residual stress and impact performance differ from the printed values by an amount the sheet does not quantify.

Shot size to cylinder volume of 30 to 70 percent keeps residence time within the resin’s thermal tolerance. For the thermally conductive grades Covestro states the same idea as a shot length of two to three times the screw diameter, and it shows what happens when material sits for about an hour at molding temperature: residue builds on the screw flights and check ring, the screw may no longer rotate and the nozzle can clog.

  • Melt temperature. The sheet’s lower bound is 280 °C and its upper bound 320 °C, with 300 °C as the standard. For the conductive grades Covestro states that the best melt temperature balances filling against localized mold heating.
  • Residence time. Material that sits at molding temperature builds residue on the screw and check ring, as the TC sheet’s photograph of a seized screw shows.
  • Mold temperature. The sheet allows 80 to 120 °C. Covestro’s TC sheet reports little effect of mold temperature on flow length for those grades and a sticking problem when the mold is too hot.
  • Venting. The vent depth of 0.025 to 0.075 mm (0.001 to 0.003 in) is a fine feature that a toolmaker cuts and checks deliberately.

Wall Thickness, Flow Length and Thermally Conductive Polycarbonate

Polycarbonate fills thin walls at the price of pressure, and Covestro’s processing sheet for Makrolon TC gives the cleanest published statement of the trade. For those thermally conductive grades the minimum practical nominal wall is 1.5 mm (0.059 in), and the sheet reports that studies show increasing wall thickness from 1.5 to 2.0 mm (0.059 to 0.079 in) lengthens the flow path by 50 to 100 percent depending on processing conditions and grade. It recommends a minimum rib thickness of 1.5 mm with adequate venting at the apex of the draft angle.

Makrolon TC629 is the grade the sheet names for the highest thermal conductivity, rated at 8 W/m·K or more for select grades. Its suggested melt range is 300 to 350 °C (572 to 662 °F) with the ideal at 310 to 330 °C (590 to 626 °F), higher than general-purpose polycarbonate because the filled melt freezes fast. Mold temperature is 65 to 100 °C (150 to 212 °F), and values of 65 to 82 °C (150 to 180 °F) avoid sticking, while excessive mold temperature produces slight delamination, sticking and residue on the tool. Back pressure runs 5.5 to 7 MPa (800 to 1,000 psi) with a screw speed of 70 to 100 rpm, and regrind to 20 percent had little effect on conductivity in the maker’s studies.

Why the TC sheet matters for a clear-grade buyer

A buyer who never orders a conductive grade can still take three lessons from it. Wall thickness controls fill in polycarbonate more than any setting on the machine. Higher melt temperature lengthens the flow, but the sheet cautions that excessive heat causes localized heating of the mold, sticking and difficult ejection. And beryllium copper inserts are suggested for ribs and deep cores where sticking occurs, since high-conductivity mold materials remove heat from exactly those places.

The first lesson is the one to carry into design. A part with a 1.2 mm wall at the end of a 150 mm flow path is a different molding problem from the same part at 2.0 mm, and the second version is the one that fills with a hold pressure in the range of Table 2.

Polycarbonate Shrinkage and Dimensional Expectations

Mold shrinkage for Makrolon 2407 is 0.65 percent parallel to the flow and 0.7 percent normal to it, measured on a 60 by 60 by 2 mm plaque at a hold pressure of 500 bar (50 MPa, 7,250 psi) under ISO 294-4. A second line on the sheet gives a practical range for parts of 0.5 to 0.7 percent under ISO 2577, based on general practical experience, and Covestro adds in its footnotes that actual production values vary with part and mold design and with molding conditions.

The two numbers, 0.65 and 0.7, are close, which is the character of amorphous resin. Orientation exists, but the difference between flow and cross-flow is 0.05 points, where a glass-filled nylon 66 from BASF differs by 0.64 points on the same ISO test. A clear polycarbonate part therefore keeps its proportions when it shrinks, and the issue is the 0.5 to 0.7 spread in practice.

On a 100 mm dimension the nominal shrinkage of 0.65 percent removes 0.65 mm, and the practical range of 0.5 to 0.7 percent covers 0.50 to 0.70 mm. If a cavity were cut for 0.6 percent, at 100.60 mm, the part would measure 100.10 mm at the low end of the range and 99.90 mm at the high end. That spread of 0.2 mm on 100 mm is the tolerance that shrinkage uncertainty alone imposes before gate position, wall thickness or tool wear are counted.

Thermal expansion adds another 0.65E-4 per K. Over the 23 to 55 °C interval the sheet cites, a 100 mm length grows 0.21 mm, so a gauge reading taken on a warm part is not a gauge reading taken at 23 °C.

Creep, Yield and Long-Term Load in a Molded Polycarbonate Part

A datasheet’s short-term modulus overstates what a loaded part keeps for months. The Makrolon 2407 sheet prints the tensile creep modulus at 2,200 MPa (319,000 psi) after 1 hour and 1,900 MPa (276,000 psi) after 1,000 hours under ISO 899-1, a fall of 14 percent over the span, against a short-term tensile modulus of 2,400 MPa. A snap hook or screw boss that carries a steady load is designed on the lower figure, and the lower figure is itself a value for a bar at 23 °C.

The same sheet shows why polycarbonate is chosen for toughness. Yield stress is 66 MPa (9,600 psi) at a yield strain of 6.0 percent, nominal strain at break is above 50 percent, and stress at break is 65 MPa (9,400 psi) with a strain at break of 120 percent, all under ISO 527-1, -2 at 50 mm/min. The material yields, stretches and keeps stretching, which is the opposite of the 3.6 percent strain at break of a glass-filled nylon 66 on BASF’s sheet. Polycarbonate parts tested before the tool is made are usually cut as machined plastic from extruded sheet or rod, which gives true polycarbonate in the hand but none of the flow orientation or molded-in stress a part from this resin carries.

  • A screw boss is checked for creep on the 1,000-hour modulus and for cold impact on the -30 °C Charpy value of 14 kJ/m².
  • A snap fit is sized inside the 6.0 percent yield strain, since that is where the stress-strain curve stops being elastic.
  • A clear lens is judged on stress as well as stiffness, because stress in a molded part comes from the process settings in Table 2 and cannot be read from any column of Table 1.

Properties on the sheet belong to a bar molded at 280 °C melt and 80 °C mold. A production part is molded at the conditions that fill it, and its first-article measurement is the property that counts.

Flame, Heat and Electrical Entries on the Datasheet

Polycarbonate’s printed ratings are specific to thickness, and the data sheet shows how fast they change with a thin wall.

Table 3. Burning, heat and electrical ratings printed for Makrolon 2407
Entry Condition Value
UL 94 recognized rating 0.75 mm (0.030 in) V-2
UL 94 recognized rating 2.7 mm (0.106 in) HB
Oxygen index ISO 4589-2, method A 27 %
Glow wire flammability index 0.75, 1.5 and 3.0 mm 850, 875 and 930 °C
Glow wire ignition temperature 0.75 to 3.0 mm 875 °C
Relative temperature index, tensile strength 1.5 mm, UL 746B 125 °C
Relative temperature index, tensile impact 1.5 mm, UL 746B 115 °C
Comparative tracking index solution A, IEC 60112 250
Electrical strength 1 mm, IEC 60243-1 34 kV/mm
Volume resistivity IEC 62631-3-1 1E14 ohm·m

This general-purpose grade is V-2 at 0.75 mm and HB at 2.7 mm. A buyer who needs V-0 in a thin wall names a flame-retardant polycarbonate grade, not this one, and the UL 94 rating belongs to the grade, thickness and color recorded for it.

Covestro’s disclaimer on the sheet states that the product is not designated for the manufacture of a medical device or its intermediates, and not for food contact or cosmetic applications. Any such use is a matter for the grade’s maker and for the purchaser’s own determination, and the sheet asks that Covestro be contacted in advance for an agreement to sell for those purposes.

Polycarbonate in an Aluminum Injection Mold

Aluminum conducts heat well, and polycarbonate arrives hot. The trade literature on aluminum tooling points to a larger process window than steel because of the thermal advantages, with the caution that excessive temperature and injection pressure damage an aluminum tool by shifting detail and galling. A melt at 300 °C and a mold at 80 to 100 °C sit inside what an aluminum tool is built for, but the pressure at the gate is the toolmaker’s number, not the resin’s.

Two features of this resin matter at the tool. Venting at 0.025 to 0.075 mm is a fine feature, and the trade article on aluminum tools asks for a wear and galling check every time the tool leaves the press, which covers vents along with gates and shutoffs. Surface finish matters because the molded surface copies the cavity surface, so a clear part is only as clear as the polish it was molded against. The sources opened for this piece do not state which polish grade a given aluminum alloy accepts or how long it holds, so that question goes to the toolmaker with a sample plate.

  • Pressure. Hold at 50 to 75 percent of injection pressure, and agree the allowable cavity pressure before the first shot.
  • Cleaning. Take the tool apart after each run and check gates, vents and shutoffs.
  • Dryness. The pellet at 0.02 percent moisture or below is a process control agreed in advance, not a datasheet footnote.

Polycarbonate gives a tough, clear and heat-tolerant part from the cheapest class of tool, provided the pellet is dry, the walls are chosen for the flow length and the shrinkage range is written into the first-article plan. For programs between a handful and a few thousand parts, low-volume injection molding is the working form of bridge production.

Sources and Further Reading

Request an Injection Molding Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Injection Molding chosen.

Request a Quote