A round lid 305 mm (12 in) across and 1.5 mm (0.06 in) thick, simulated in MoldMaking Technology’s article on volumetric shrinkage, left the mold with local volumetric shrinkage anywhere from 2.4 % to 11.8 %. The wall was uniform. Packed at one pressure until ejection, the outer rim shrank more than the region near the gate, and like a plate squeezed at its edge, the middle domed.
Every molded part shrinks unevenly, and warpage is what that unevenness does to the shape once the steel stops holding it. A flatness tolerance is the drawing’s answer, but it only means something when the drawing also says how the part is held, at what temperature and how long after molding it is measured. This piece traces warpage to its causes as the simulation and resin makers describe them, and sets out how flatness is written so that the molder and the inspector read the same number.
How Warpage Relates to a Flatness Tolerance
Autodesk’s Moldflow help defines the cause in one line: warpage comes from variations in shrinkage. Plastics Technology’s article on the causes of warpage puts it the same way. A part that shrinks uniformly in every direction becomes smaller but keeps its shape, and a part in which one region shrinks more than another carries internal stress that bends or twists it on ejection.
A flatness tolerance limits the result. It is one of the form tolerances whose symbols and rules of interpretation are defined in ISO 1101, which its scope describes as the symbol language for geometrical specification of workpieces. ISO 20457, the tolerance standard for plastic molded parts, works through general tolerances given as a surface profile tolerance within a datum system, and allows further geometrical specifications where function requires them. A flatness callout on a molded face is one of those additions.
The condition of measurement matters as much as the number. ISO 10579 exists for parts that deflect under their own weight or under light force: its scope covers dimensioning and tolerancing non-rigid parts where features have to be restrained during verification. A thin molded cover can read one flatness lying free on a table and another clamped at its screw bosses.
Warpage is uneven shrinkage released at ejection. A flatness callout limits it only when the drawing also states whether the part is measured free or restrained, and when.
Where Uneven Shrinkage Comes From
The Plastics Technology article lists five common reasons for shrinkage to vary across a part:
- Cooling rate. Faster cooling leaves semi-crystalline resins less time to crystallize, which lowers their volumetric shrinkage; the effect is smaller for amorphous resins.
- Orientation. Shear during filling aligns molecules or fibers with the flow. Amorphous resins relax and shrink more along the flow; semi-crystalline resins crystallize more across it and shrink more in that direction.
- Mold restraint. In the mold the part cannot shrink within its surface, only through its thickness, so stresses build in the plane and relax after ejection. Materials that resist creep and relax more slowly show higher linear shrinkage.
- Mold temperature difference. A cavity side hotter than the core side lets one face shrink more, which bends the part.
- Wall thickness and distance from the gate. Thick areas cool longer and shrink more; areas far from the gate are less densely packed than areas near it.
Fibers change the direction of the effect. Plastics Technology notes that glass fibers do not shrink with temperature, so a fiber-filled resin shrinks less along the fiber direction. MoldMaking Technology puts the difference at 2 to 10 times less shrinkage along the fibers than across them, and advises against a single mold shrinkage value for such materials. DuPont’s Zytel guide says the same for glass-reinforced nylon: mold shrinkage is always lower in the flow direction and close to that of unreinforced nylon across it.
The datasheets show how much the direction matters for unreinforced resins. Shrinkage measured under ISO 294-4 on a 60 × 60 × 2 mm plaque is printed parallel and normal to flow, and the difference between the two is the raw material of warpage on a flat part.
| Material | Parallel | Normal | Difference on 100 mm (3.94 in) | Source and test |
|---|---|---|---|---|
| Polycarbonate, Makrolon 2407 | 0.65 % | 0.7 % | 0.05 mm (0.002 in) | Covestro datasheet, ISO 294-4, 500 bar |
| PC+ABS, Bayblend T85 X | 0.55 to 0.75 % | 0.55 to 0.75 % | No directional difference printed | Covestro datasheet, ISO 294-4, 500 bar |
| PC+ABS, Bayblend RW85 XF | 0.6 to 0.8 % | 0.6 to 0.8 % | No directional difference printed | Covestro datasheet, ISO 294-4 |
| Polypropylene, generic | 1.8 to 2.5 % | flow and cross-flow differ by under 0.2 % | Under 0.2 mm (0.008 in) | Autodesk Moldflow PP materials page |
| Polypropylene with 30 % glass | About 0.7 % | Not given | Not given | Autodesk Moldflow PP materials page |
Covestro adds a caution to its shrinkage rows: they come from plaques molded under controlled conditions, and production parts vary. The table shows what the resin brings, not what a given part will do.
Volumetric Shrinkage and the Packing Profile
Mold shrinkage and volumetric shrinkage answer different questions, and MoldMaking Technology’s article separates them. Mold shrinkage, typically 0.5 to 2 %, says how much larger to cut the cavity. Volumetric shrinkage says how evenly and how well the part is packed, and on a well designed part, tool and process its average maximum at ejection is around 8 %. A cube 2 % smaller in each direction is about 6 % smaller in volume, which is why volumetric figures look three times larger.
The lid in the opening shows the mechanism. With a single packing pressure held until ejection, the rim far from the gate shrank more than the center. The article reports that a packing profile that varies pressure over time, matched to how the part freezes, made volumetric shrinkage more uniform, and the part warped less and came closer to its dimensions.
Autodesk’s Moldflow Shrink analysis is built on the same idea from the mold maker’s side. It uses shrinkage data measured on the material under a range of processing conditions to recommend one shrinkage allowance for cutting the cavity, shows whether that single value is valid across the part, and, where critical dimensions and tolerances are defined, predicts whether they can be met in X, Y and Z. Its Warp analysis diagnoses the cause and recommends changes to gate location, design parameters or wall thickness variation.
Mold shrinkage sizes the cavity. Volumetric shrinkage, and how evenly it is spread, decides whether the part comes out flat.
Mold Temperature, Cooling and Ejection
BASF’s troubleshooting brochure gives five process and design causes for warpage. Mold temperatures may be unfavorable, and different temperatures on the two mold halves or on sliding cores can correct it, mainly for unreinforced resins. Walls of different thickness need redesign. A pressure gradient too steep along the flow path can be eased with more gates, again for unreinforced resins. A cooling time too short ejects the part hot enough to deform, so cooling is lengthened and the part is checked for catching on negative draft. And the material itself may be the cause, in which case a low-warpage grade such as a blend with an amorphous phase narrows the gap between lengthwise and crosswise shrinkage.
The brochure illustrates the mold temperature point with three settings on one part. With cavity and core both at 80 °C (176 °F), the printed play was −1.4. With the core at 30 °C (86 °F), it was +2.6, and with the core at 50 °C (122 °F), +0.4. The brochure does not print a unit for the play, but the signs show the warp reversing as the core is cooled and passing close to zero between the two settings.
DuPont’s Zytel guide names the same mechanism for nylon. Non-uniform mold temperature, local overheating of cores or a missing water channel in one area of the cavity changes the crystallization rate locally, and with it the shrinkage.
Warpage That Appears After Molding
Not all warpage is present at ejection. Suhas Kulkarni’s Plastics Technology series on post-mold shrinkage explains that molecules keep moving toward their final positions while they are above their glass transition temperature. For a resin whose glass transition is below room temperature, shrinkage continues on the shelf. He describes a TPE overmolded on a metal insert that had not finished shrinking after 96 hours and needed seven days.
Low mold temperature adds a second delay. A molder may run the mold colder to hit dimensions, shorten the cycle, reduce flash or improve flatness, but the molecules freeze before they reach their positions and the part carries stress that inspection does not see. Heat releases it later. Kulkarni’s example is a cassette that warped after a few days in a parked car, where the inside can reach 65 °C (150 °F), and he notes that warehouses and trucks that are not temperature controlled can do the same to parts that will never see heat in service.
Semi-crystalline resins add incomplete crystallization. In his DSC example, a nylon molded with the mold at 82 °C (180 °F) reached an estimated 31.5 % crystallinity, and at 32 °C (90 °F) only 20.9 %. The missing crystallization can resume when the part is warmed, with shrinkage and warpage following. Annealing in an oven before assembly lets the molecules settle, and parts assembled together should have been through the same post-mold history.
| Item | Value | Source and condition |
|---|---|---|
| Time for a TPE overmold to finish shrinking | Over 96 h, about 7 days | Plastics Technology, one project |
| Temperature inside a parked car | Up to 65 °C (150 °F) | Plastics Technology |
| Nylon crystallinity, mold at 82 °C (180 °F) | 31.5 % | Plastics Technology, DSC estimate |
| Nylon crystallinity, mold at 32 °C (90 °F) | 20.9 % | Plastics Technology, DSC estimate |
| Polycarbonate tensile creep modulus, 1 h | 2,200 MPa (319,000 psi) | Makrolon 2407 datasheet, ISO 899-1 |
| Polycarbonate tensile creep modulus, 1,000 h | 1,900 MPa (276,000 psi) | Makrolon 2407 datasheet, ISO 899-1 |
| Polycarbonate short-term tensile modulus | 2,400 MPa (348,000 psi) | Makrolon 2407 datasheet, ISO 527 |
The creep rows matter for parts that are flattened in assembly. A housing screwed flat against a frame is held at a fixed deflection, and the stress needed to hold it falls as the material creeps. Covestro’s sheet shows polycarbonate’s creep modulus dropping from 2,200 MPa (319,000 psi) at 1 hour to 1,900 MPa (276,000 psi) at 1,000 hours, about 14 % lower, against a short-term tensile modulus of 2,400 MPa (348,000 psi). A part pulled flat by its fasteners therefore relaxes into its new shape partly, and a flatness measured restrained on day one does not describe the part when it is unbolted a year later.
Design and Gating Against Warpage
The cheapest flatness is designed in. DuPont’s Zytel guide asks for uniform wall thickness, cored-out thick sections and shapes that can shrink without restraint. For glass-reinforced nylon it recommends center gating of round parts, full edge gating of thin rectangular or square parts under 1.5 mm (0.06 in), gating long parts so the melt strikes a core or wall, and gates about 50 % larger than for unreinforced nylon. Any condition that randomizes the fibers, such as abrupt changes of flow direction or multiple gates, reduces warpage.
BASF’s rules for glass-fiber resins point the other way, toward a uniform orientation rather than a random one. Its list for optimizing warpage reads:
- Gate so that the flow direction, and so the orientation, is uniform.
- Gate elongated parts lengthwise; symmetrical parts are best.
- Avoid ribs or walls perpendicular to the flow direction.
- Place the end of the flow path in corners where possible.
- Aim for abutting weld lines, keeping their strength in mind, and keep them off exposed webs.
The two guides are not in conflict. Both aim to remove the difference in orientation from one area to another, one by making it random everywhere and the other by making it the same everywhere. Simulation of the fiber orientation, which BASF recommends, shows which one a given part can reach.
When a part still warps, the cavity can be cut to the opposite shape. MoldMaking Technology’s article on warpage compensation describes mapping points on the simulated warped part back onto the original model, so that the steel is cut pre-bent and the part relaxes toward nominal. The article warns that the method moves holes, drafts and parting lines with it, so features have to be realigned and draft directions held, and a complicated model may need more than 100 point pairings.
Writing Flatness on the Drawing
A flatness requirement on a molded part is clearest when it carries its conditions with it. These are the items the sources point to:
| Element | What it settles | Basis |
|---|---|---|
| The form tolerance and its value | The zone the surface has to fall within | ISO 1101 symbol language |
| The datum system for the rest of the part | Where general tolerances are read from | ISO 20457, surface profile within a datum system |
| Free state or restrained, and how | Whether clamping at bosses or edges is allowed during the check | ISO 10579, non-rigid parts |
| Measuring temperature | Size and shape at the gauge | Covestro datasheets give properties at 23 °C (73 °F) |
| Time after molding or annealing | Whether post-mold shrinkage has finished | Plastics Technology, post-mold shrinkage |
Henz’s column in Plastics Technology gives a reference point for how much bow many parts tolerate: 0.13 to 0.38 mm (0.005 to 0.015 in) of bow or out-of-roundness is acceptable on many designs, and a part that cannot accept it needs its gate placed for straightness or roundness. That range is a description of common parts, not a standard class, and the paid tables of ISO 20457 were not opened for this piece.
The checks follow from the table. Measure first samples free and, if the drawing allows, restrained as specified. Measure them again after the post-mold period the resin needs, at the stated temperature. Where a part is flat only when restrained, read the creep figures for the resin before relying on assembly to hold it.
A flatness number is complete with four conditions: the datum, free or restrained, the temperature and the time since molding.
For a bridge tool, flatness is the property most likely to move between the first shots and the run, because packing profile, mold temperature balance and post-mold time all reach it. In low-volume injection molding for bridge production, the conditions in Table 3 are agreed with the first article, so that a flat part on the bench stays flat in the box.
Sources and Further Reading
- Warp analysis (Concept), Moldflow 2015 help, Autodesk
- Shrink analysis (Concept), Moldflow 2015 help, Autodesk
- PP materials, Moldflow 2015 help, Autodesk
- Injection-Molding Problems in Engineering Thermoplastics, Causes and Solutions, BASF
- Zytel and Minlon Nylon Resins Molding Guide, 2017, DuPont
- Makrolon 2407 ISO Datasheet, edition 18 September 2023, Covestro
- Bayblend T85 X Technical Datasheet, version 2026-07-02, Covestro
- Bayblend RW85 XF ISO Datasheet, edition 19 September 2023, Covestro
- ISO 1101:2017 Geometrical product specifications, Geometrical tolerancing, record and scope, EVS
- ISO 10579:2010 Dimensioning and tolerancing of non-rigid parts, record and scope, EVS
- ISO 20457:2018 Plastics moulded parts, Tolerances and acceptance conditions, record and scope, SIS
- Injection Molding, The Causes of Warpage, Plastics Technology
- Understanding Postmold Shrinkage, Why Part Dimensions Change Over Time, Part 2, Plastics Technology
- Don’t Overlook Gate Location, Plastics Technology
- Use Volumetric Shrinkage Predictions to Improve Part Quality, MoldMaking Technology
- From Shrinkage to Simulation, Mastering Warpage Compensation in Mold Design, MoldMaking Technology