A deep pattern texture can reach 0.18 mm (0.007 in). Under the rule of thumb many design guides still print, 1.5° of draft for every 0.025 mm (0.001 in) of texture, that texture asks for 10.5° on each side wall, and a cup drawn with a 5° opening would need a 21° one. Boulder Engineering Studio used that cup to show how late a texture choice can wreck a finished design. The texture maker behind the most widely specified texture library now says the 1.5° rule itself is too generous to rely on.
Texture adds small undercuts to every wall it covers. When the part shrinks and the mold opens, those peaks and valleys drag along the steel unless the wall leans away from the direction of pull. This piece sets out the draft that texture depth calls for, the conditions under which each figure holds, how the mold surface is prepared before texturing and how depth and finish are checked on the part.
How Much Draft a Texture Depth Needs
Standex Engraving Mold-Tech’s technical data sheet gives the current recommendation from the texture maker: 1° of draft for every 0.013 to 0.015 mm (0.0005 to 0.0006 in) of texture depth. Per 0.025 mm (0.001 in) that works out to between 1.7° and 2°. The same sheet states that the typical figure of 1.5° per 0.025 mm (0.001 in) “is no longer a valid guideline”, given newer molding materials, molding parameters and complex mold designs.
Two other figures are in circulation. MoldMaking Technology’s article on texturing for thermoplastics gives a minimum of 1° per side for every 0.025 mm (0.001 in), and warns that below it the part risks drag marks. Boulder Engineering Studio’s design note uses 1.5° per 0.025 mm (0.001 in) and lists three Mold-Tech textures on that basis: MT-11010 at 0.025 mm (0.001 in) needing 1.5° or more, MT-11020 at 0.038 mm (0.0015 in) needing 2.25° or more, and MT-11030 at 0.051 mm (0.002 in) needing 3°.
| Texture depth | Minimum rule, 1° per 0.001 in (MoldMaking Technology) | Older rule, 1.5° per 0.001 in (Boulder) | Mold-Tech current rule, 1° per 0.0005 to 0.0006 in (Standex) | Shrink-on wall, 2 to 3 times the Mold-Tech figure |
|---|---|---|---|---|
| 0.013 mm (0.0005 in) | 0.5 | 0.75 | 0.8 to 1.0 | 1.7 to 3.0 |
| 0.025 mm (0.001 in) | 1.0 | 1.5 | 1.7 to 2.0 | 3.3 to 6.0 |
| 0.038 mm (0.0015 in) | 1.5 | 2.25 | 2.5 to 3.0 | 5.0 to 9.0 |
| 0.051 mm (0.002 in) | 2.0 | 3.0 | 3.3 to 4.0 | 6.7 to 12.0 |
| 0.076 mm (0.003 in) | 3.0 | 4.5 | 5.0 to 6.0 | 10.0 to 18.0 |
| 0.102 mm (0.004 in) | 4.0 | 6.0 | 6.7 to 8.0 | 13.3 to 24.0 |
The columns are each source’s rule applied to the same depths; only the Boulder figures at 0.025, 0.038 and 0.051 mm are printed values. The rule’s “per side” matters. Draft is measured on each wall against the line of draw, so a cup’s included opening angle is twice the per-side figure.
Read across a row, the spread is large. At 0.051 mm (0.002 in), a wall drawn to the minimum rule has 2°, and the texture maker’s figure is 3.3° to 4°. A wall designed for the old 1.5° rule falls short of the current Mold-Tech recommendation at every depth.
Texture draft is now best read from the texture maker’s sheet: about 1.7° to 2° per side for each 0.025 mm (0.001 in) of depth, on a wall the part shrinks away from.
Why the Mold-Tech Figure Moved
Standex gives three reasons in a single sentence: new molding materials, new molding parameters and complex mold design elements. It does not name the materials. What the sheet does make explicit is the list of things that decide whether a textured part releases: part design, part size, molding material, texture construction and molding parameters.
Texture construction is the term that separates one texture from another at the same depth. MoldMaking Technology’s article describes how chemical-etch textures are made by masking the steel and exposing it to ferric chloride or nitric acid, either flowed over the block or by dunking it. Spray patterns, where the resist is sprayed on, are the cheapest and closely resemble EDM finishes. Transfer patterns are applied from sheets and can be layered into multi-depth grains, which look more natural and take more handwork where sheets meet on contours.
A texture with sharp peaks grips the steel differently from one whose edges have been broken. The same article describes a “round off” step, an open etch with all resist removed, that softens a texture that has too much edge. The depth number alone does not capture that difference, which is one reason the texture maker asks to be consulted early.
Shrink-Away Walls, Shrink-On Walls and Shut-Offs
Every figure in Table 1 is for one condition. Standex states that its rule is specific to shrink-away side walls, where the cooling part pulls away from the steel. Areas where the part shrinks onto the steel need 2 to 3 times as much draft.
MoldMaking Technology’s article on engraving cores and cavities describes the same split. As the plastic cools in the mold it shrinks away from the cavity wall and toward the core, so a shallow engraving in the cavity usually releases without trouble. On the core side, the part grips the steel as it shrinks, and the draft has to overcome that grip as well as the texture.
Three more conditions from the Standex sheet extend the list:
- Lifters, slides and other moving components are judged by their own angle of action in the tool, not by the main line of draw.
- Shut-offs on textured side walls need additional draft or special work for the part to release cleanly.
- Texture depth can be reduced locally, without a visible hard line, where a full-depth texture would cause ejection trouble.
Boulder’s note adds the shut-off figure from the mold’s side. Where core and cavity steel slide against each other, as at the hole under a snap fit, the steel needs around 3° to 5° of draft to limit wear, with 3° described as a good value. A snap fit with a light 0.025 mm (0.001 in) texture needs only 1.5° on its visible faces by the older rule, but the hole beneath it is drawn oversize so that the shut-off can have 3°.
Draft depends on which way the part shrinks. A shrink-on wall takes two to three times the figure for a shrink-away wall, and a moving component takes its draft from its own direction of travel.
Draft on Smooth Walls as the Baseline
Texture draft is added to the draft the wall would need anyway. DuPont’s molding guide for Zytel nylon gives 0.5° to 1° per side as usually satisfactory for its resins on ribs, bosses and side walls, and up to 2° per side for softer, more elastic resins.
Engraved lettering and logos are the shallow end of the same question. MoldMaking Technology’s engraving article recommends that engravings be no deeper than 0.25 mm (0.01 in), with a width of 1.5 to 2 times the depth. Molded-in lettering is legible from eight points, and six in exceptional cases, at a depth of 0.08 to 0.13 mm (0.003 to 0.005 in). On cavity side walls it suggests a maximum of 0.1 mm (0.004 in), or less in difficult cases, and engraving on the side of a core at about 0.1 mm, with less where the draft is under 1°.
| Feature | Depth | Condition |
|---|---|---|
| Any engraving | Up to 0.25 mm (0.01 in) | Width 1.5 to 2 times the depth |
| Molded-in lettering | 0.08 to 0.13 mm (0.003 to 0.005 in) | Eight point minimum, six in exceptional cases |
| Engraving in a cavity side wall | Up to 0.1 mm (0.004 in), less for difficult cases | Depends on draft, wall thickness and resin |
| Engraving in a core side wall | About 0.1 mm (0.004 in), less below 1° of draft | Part shrinks onto the core |
Where an engraving or texture is too deep for the draft available, the article names the alternatives: side cores in the cavity or split cavities. Both need more space and a larger mold, and both can add scrap and cycle time.
Preparing the Mold Surface for Texture
A texture reproduces whatever surface lies under it. Standex recommends a 500 emery finish for textures shallower than 0.020 mm (0.0008 in), 400 emery for textures from 0.020 to 0.10 mm (0.0008 to 0.004 in), and 320 emery for textures deeper than 0.10 mm (0.004 in). The MoldMaking Technology article treats an SPI B-3, 320 paper finish as a safe preparation and warns that patterns 0.025 mm (0.001 in) deep will show cutter marks.
| Texture depth | Prepared finish |
|---|---|
| Under 0.020 mm (0.0008 in) | 500 emery |
| 0.020 to 0.10 mm (0.0008 to 0.004 in) | 400 emery |
| Over 0.10 mm (0.004 in) | 320 emery |
| Any depth | Free of EDM, cutter marks, burns and EDM scale |
The EDM condition in the last row is strict for a reason. The MoldMaking Technology article explains that EDM leaves a white, recast layer, chemically altered from the parent steel, which does not etch uniformly and typically will not take plating or nitriding either. Hard-milled surfaces carry uneven work hardening that etches unevenly. Welds need proper preheat and post-heat, or the weld zone shows through the texture as a ring.
Steel type matters too. Aluminum etches faster than steel and the reaction gives off heat, so the bath temperature has to be controlled, and cast aluminum can show pores deeper than the texture itself. Martensitic 420 stainless is easier to texture than the 300 series, but a 420 block hardened to 52 to 54 HRC takes longer than one at 40 HRC. Standex lists P-20, H-13, S-7, O-1, A-1, A-2, A-6, 420 stainless, beryllium copper, kirksite and forged and cast aluminum among the tool materials it has textured.
How Texture Depth and Draft Are Checked
Texture is usually controlled by eye against a reference sample, and the MoldMaking Technology article on textured molds suggests going further: silicone replicas of the textured surface and profilometers to measure texture depth and roughness. Draft can be read from the part model and from the mold, but whether the texture releases is seen on the part, as drag marks or scuffing on the walls.
Gloss is the other measured property of a textured surface. Standex notes that gloss on a molded part is read with a 60° gloss meter, and that it depends on molding material, tool temperature, pack pressure, melt temperature, venting, cycle time, wall thickness, flow, texture pattern and mold coatings. The MoldMaking Technology article reports, for textured automotive TPO parts, that a 60° gloss of at least 2.2 is often taken as the threshold for marring resistance, and that medium grains of 0.051 to 0.076 mm (0.002 to 0.003 in) hide surface marks while staying fine in appearance. That finding is specific to TPO and to parts still under test.
The checks that follow from the sources are these:
- The texture is named with its number and, if it is not the default, its depth.
- Draft on every textured wall is read against the texture maker’s figure for that depth, and doubled or tripled where the part shrinks onto steel.
- The mold surface is free of EDM scale and cutter marks and finished to the emery grade for the depth.
- First parts are inspected for drag marks and scuffing on textured walls, and gloss is read with a 60° meter where it is specified.
- Where draft is short, the texture depth is blended down locally rather than left to scuff.
A texture number without a depth is filled in by the texture house with its default depth. The draft on the drawing has to match whatever depth the texture house will actually cut.
Keeping Texture Depth Through a Run
Draft that suits a fresh texture also has to suit a worn one. MoldMaking Technology’s article on surface texture quality notes that as tooling wears, the depth and sharpness of an etched finish degrade, and that judging by eye whether parts are still close enough to the reference is open to interpretation. Measured texture depth gives a number that can be tracked against shot count, and a depth limit set from wear data tells when the mold needs rework.
Release agents work against texture in a different way. The article on textured molds advises using them sparingly and checking compatibility, because overuse builds up in the grain and changes the texture the part receives. It recommends nonabrasive cleaning, frequent inspection for early wear, restoration of worn texture by laser etching or other professional methods, and no overpolishing, which erodes detail.
Damage needs the same care. Standex asks that a damaged textured mold not be repaired in the shop, and that the texture house receive photographs of the mold and the damaged area, the steel type, the texture number, the part name, the date of texturing and the texture location. Before texturing, its preparation list asks for the mold to be disassembled, only the components to be textured shipped, flat shut-offs scribed clearly and all EDM scale and cutter marks polished out.
The same textured article recommends naming the exact texture designation from the chosen texture house and avoiding “or equivalent”, since textures from different masters do not match. Sample plaques molded in the specified material let the texture, its feel and its release be judged before the production tool is etched.
Writing Texture and Draft on the Drawing
MoldMaking Technology’s texturing article makes one drawing point plainly. Each standard texture has a default depth, and a texture specified without a depth callout is cut to that default. A drawing that names a texture therefore fixes a depth, and with it a minimum draft, whether or not the depth is written.
The simplest protection is to choose the texture before the side walls are final, read its depth from the texture maker and set the per-side draft from Table 1 with the Mold-Tech figure, then double check the shrink-on faces, slides and shut-offs. Where the part cannot take the draft, the texture can be blended shallower in that area or moved to a face that does not slide.
On a short-run tool the texture is often the last step before sampling, which is late to discover that a wall is short of draft. A part with walls drawn to the old 1.5° rule may still release, but the texture maker’s own figure is the one to design to when low-volume injection molding has to carry a textured part from the first shots into bridge production without scuffed walls.
Sources and Further Reading
- Texture Technical Data Sheet, Standex Engraving Mold-Tech
- Texturing Molds for Thermoplastics, Factors for Success, MoldMaking Technology
- How To Master Textured Molds With Design and Quality Control, MoldMaking Technology
- Best Practices for Engraving Cores and Cavities, MoldMaking Technology
- How to Assess and Control Surface Texture Quality, MoldMaking Technology
- The Subtleties of Draft Angles and Injection Molding, Boulder Engineering Studio
- Zytel and Minlon Nylon Resins Molding Guide, 2017, DuPont