SPI Mold Finish Grades A-1 to D-3 for Injection Molded Parts

The SPI finish grades read for a buyer, with what each method gives, how texture costs draft, and how a finish is written and kept on an aluminum tool.

Four injection molded black plastic plaques with different surfaces, mirror gloss, satin, fine matte and coarse matte.

DME, which makes mold components and finishing supplies, prints the SPI finish grades with the roughness each one approximately leaves on the steel: 0 to 1 µin (0 to 0.025 µm) Ra for A-1, a diamond-buffed mirror, and 190 to 230 µin (4.8 to 5.8 µm) for D-3, a coarse oxide blast. Between those two ends sit ten more grades, each a way of finishing the cavity steel that a drawing can name in three characters.

The SPI scale is the one finish vocabulary that molders, toolmakers and buyers share without translation. This piece reads the twelve grades from DME’s guide, shows what a molded part takes from each, and sets out where texture depth and draft meet, using the texture maker’s own current rule. The Society’s own comparison standard was not opened for this piece, and the Ra values carry the approximate character DME gives them.

What the Twelve SPI Finish Grades Specify

The SPI system names a finish by a letter and a number. Its letter gives the finishing method, A for diamond buff, B for grit paper, C for stone and D for dry blast, while the number runs from 1, the finest within a letter, to 3, the coarsest. DME’s guide gives each grade its preparation and an approximate resulting Ra in microinches, and for the blasted grades it prints the blast conditions as well.

Table 1. SPI mold finish grades with preparation and approximate resulting Ra, from DME’s Micro-Finish Mold and Tool Finish Guide
Grade Preparation Ra (µin) Ra (µm)
A-1 Grade #3 diamond buff 0 to 1 0 to 0.025
A-2 Grade #6 diamond buff 1 to 2 0.025 to 0.051
A-3 Grade #15 diamond buff 2 to 3 0.051 to 0.076
B-1 600 grit paper 2 to 3 0.051 to 0.076
B-2 400 grit paper 4 to 5 0.10 to 0.13
B-3 320 grit paper 9 to 10 0.23 to 0.25
C-1 600 stone 10 to 12 0.25 to 0.30
C-2 400 stone 25 to 28 0.64 to 0.71
C-3 320 stone 38 to 42 0.97 to 1.07
D-1 Dry blast, glass bead #11, 8 in (203 mm) at 100 psi (6.9 bar), 5 s 10 to 12 0.25 to 0.30
D-2 Dry blast, #240 oxide, 5 in (127 mm) at 100 psi, 6 s 26 to 32 0.66 to 0.81
D-3 Dry blast, #24 oxide, 6 in (152 mm) at 100 psi, 5 s 190 to 230 4.8 to 5.8

The micrometer column is converted from DME’s microinches by multiplying by 0.0254. Three features of the table are worth reading before a grade is chosen.

First, A-3 and B-1 share one Ra range, 2 to 3 µin, although one is diamond buffed and the other is finished with 600 grit paper. A single roughness average cannot tell the two apart, which is why the grade, not the Ra value, is the statement a drawing needs. Paper finishing and diamond buffing are different operations, and one roughness average records neither.

Second, the scale is not a ladder of roughness. D-1, a glass-bead blast, lands at 10 to 12 µin, the same as C-1 and finer than C-2 and C-3. A blasted satin surface and a stoned surface can carry the same Ra and look nothing alike, because one is a field of small craters and the other a set of directional scratches. The letter is the half of the grade that says which.

Third, the steps are uneven. B-2 tops out at 5 µin and B-3 starts at 9; C-1 ends at 12 and C-2 starts at 25; D-2 ends at 32 and D-3 starts at 190. The grades are steps in method, so a request for “something between B-2 and B-3” has no meaning on the scale.

An SPI grade names a finishing method and a result class. The Ra column describes the typical result, and a drawing that quotes only an Ra number has dropped the half of the specification that the grade carried.

DME also ties the grades to its own mold finish comparison kit, a set of physical reference plates: A-1 is comparable to plate number 1, B-3 to number 3, C-3 to number 4 and D-2 to number 5, and it notes that no current grade matches the original sixth plate. A physical plate is the kind of reference the last section of this piece recommends.

A-Grade Polish for Clear and Gloss Parts

The A grades are diamond-buffed surfaces, and they are specified when a molded part is to be seen through or when gloss is the point.

The resin sheets show why the polish carries weight for clear material. Covestro’s Makrolon 2407 polycarbonate transmits 89 percent of visible light at 1 and 2 mm, 88 percent at 3 mm and 87 percent at 4 mm, with haze below 0.8 percent at 3 mm and a refractive index of 1.584. A molded surface copies the cavity surface, so a clear part is only as clear as the finish it was molded against. The sheet’s own figures describe a bar molded in a polished tool, and a part from a B-grade cavity will not reach them.

Two process settings from the same sheet bear on the surface. The vent depth printed is 0.025 to 0.075 mm (0.001 to 0.003 in), which is 25 to 75 µm. That is a thousand times and more the Ra of an A-1 surface, and the vent is a deliberate gap in the polish that has to stay clean and shallow. The recommended mold temperature of 70 to 110 °C is the other setting the sheet gives for the cavity wall, and how much the molded surface copies from a polished wall is settled on the first samples, not on the sheet.

Gloss on a filled resin

A polished cavity does not make a glossy part from any resin. DuPont’s molding guide for nylons says reinforced resins molded with mold temperatures near 100 °C significantly improve surface finish, mold filling and surface blemishes, listed as frosting, so that a glass nylon part’s surface is set by the process at least as much as by the cavity. A buyer who specifies A-2 on a glass-filled nylon is paying for a polish that the fibers will partly undo.

  • Clear polycarbonate. A grades, with the polish checked on a sample plate before the tool is textured or coated.
  • Unfilled opaque resins. B and C grades cover most functional faces, and A-3 serves where a bright surface is needed on a visible face.
  • Glass-filled resins. A hot mold and a quick fill matter more than the A grade chosen, and a coarser grade is the one to test first where fiber marks show.

Paper and Stone Grades B and C for Functional Surfaces

The B and C grades are the working finishes of most molded parts. B-1 and B-2 are paper-finished medium polishes at 2 to 5 µin (0.05 to 0.13 µm), and B-3 steps to 9 to 10 µin (0.23 to 0.25 µm). The C grades run from 10 to 12 µin (0.25 to 0.30 µm) at C-1 to 38 to 42 µin (0.97 to 1.07 µm) at C-3.

For many parts the choice among these is about release and appearance. The table gives no draft figure for the polished and paper grades, and the choice among them is judged on a sample, not on a roughness number.

The table’s notes also say little about how a finish ages. A polish on a tool wears with every shot, and for filled resins the wear shows first at the gate and shutoffs, as the trade literature on aluminum tools says. Part appearance at shot 5,000 can differ from part appearance at shot 5, and the question to ask a toolmaker is how the finish is protected and restored, not only what it is on the day of the first shot.

D Grades, Blasted Texture and the Draft They Need

The D grades are dry-blasted surfaces, and DME prints each one as a recipe: glass bead #11 from 8 in (203 mm) at 100 psi (6.9 bar) for 5 seconds for D-1, #240 oxide from 5 in (127 mm) for 6 seconds for D-2, and #24 oxide from 6 in (152 mm) for 5 seconds for D-3. They are the satin and matte finishes seen on housings and handles. A blasted surface is a shallow texture, and every texture needs draft, because the walls of the cavity are no longer smooth and the part has to slide off them.

The texture maker has changed its rule. Standex Engraving Mold-Tech’s technical data sheet states that the typical 1.5 degrees of draft per 0.001 in (25 µm) of texture depth is no longer a valid guideline, given new molding materials, molding parameters and mold designs, and recommends 1 degree of draft per 0.0005 to 0.0006 in (12.5 to 15 µm) of texture depth. Per 0.001 in that is between 1.7 and 2 degrees.

Table 2. Draft for texture depth under Mold-Tech’s current rule, 1 degree per 12.5 to 15 µm, on a shrink-away wall (arithmetic)
Texture depth Draft, shrink-away wall Shrink-on wall, 2 to 3 times
0.001 in (25 µm) 1.7° to 2.0° 3.4° to 6.0°
0.002 in (51 µm) 3.4° to 4.1° 6.8° to 12.2°
0.003 in (76 µm) 5.1° to 6.1° 10.2° to 18.3°
0.004 in (102 µm) 6.8° to 8.1° 13.5° to 24.4°

The same sheet adds three conditions. The rule is specific to shrink-away sidewalls; areas of the tool where the part shrinks onto the steel need 2 to 3 times the draft. Lifters, slides and other moving components are judged on their angle of action in the tool. And shut-offs on textured sidewalls need additional draft or special work to release cleanly. Mold-Tech also notes that texture depth can be reduced in chosen areas without a visible hard line, which is the fix when a wall cannot carry the draft its texture asks for.

Texture costs draft, and the current rule costs more than the old one. A drawing with a blasted finish on a wall that has no draft is asking the part to slide off a surface designed to hold it.

Mold Finish on an Aluminum Bridge Tool

Aluminum tools take finishes, and the sources opened for this piece say little about how fine. The trade article from Plastics Technology on aluminum tooling discusses a nickel-boron coating about 0.0002 to 0.0003 in. (5 to 8 µm) thick that raises surface hardness to 50 to 56 HRC. It also states that the coating reduces oxidation and acts as a release agent, can be stripped and recoated, and is applied in about three days. A coating of 5 to 8 µm is several hundred times the Ra of an A-1 surface, which means the finish a molded part shows is the finish of the coated surface, and the order of polishing and coating is a question for the toolmaker.

The same article describes a four-cavity ABS tool that ran close to 200,000 shots, with the hard coat stripped and reapplied midstream when a logo was removed by machining and welding, and with the surface polished again after the weld. Where cosmetic requirements are high, the finish is a maintained surface and its maintenance appears in the tool’s plan.

Pressure and temperature in the molding window affect a finish as well, and the article warns that excessive temperature and injection pressure damage an aluminum tool through galling, and galling is damage to the cavity surface that a molded part copies. Glass-filled resin wears gates and shutoffs first, and that wear shows on the part as a changed gate vestige and flash before it shows on a polished face.

  • Name the grade and the face. A finish applies to named faces, and unnamed faces get the toolmaker’s default.
  • Name the maintenance. Say whether the finish is to be restored at cleaning or only inspected.
  • Name the sample. Agree a plate or a first sample as the reference, because a roughness number leaves the rest of the finish unspecified.

Finish Against the Other Small Dimensions on a Cavity

A finish is one of several features measured in micrometers on a cavity, and laying them side by side shows which ones compete. Every figure below comes from the tables and sheets already cited in this piece.

  • An A-1 surface averages up to 0.025 µm.
  • A paper or stone finish between B-1 and C-3 averages 0.05 to 1.07 µm.
  • A glass-bead blast at D-1 averages 0.25 to 0.30 µm, and D-3 reaches 4.8 to 5.8 µm.
  • A texture 0.001 in deep is 25 µm deep, four times the roughness average of D-3.
  • A polycarbonate vent is 25 to 75 µm deep.
  • A nickel-boron coating on an aluminum tool is 5 to 8 µm thick.

Three consequences follow. The coating is thicker than every polished, paper and stone grade is rough, so a polish applied under the coating and a polish applied over it give different surfaces, and the order has to be agreed. Vents are as deep as the shallowest textures, and a texture that reaches into a vent land changes the venting. And a texture at 0.001 in is a different order of feature from a D-grade blast, which is why the two are specified in different words, grade for a blast and texture name and depth for an etched pattern.

The finish also meets the part at the gate. A gate vestige is a small area of a different surface, where the melt entered and the gate was cut or broken off. No SPI grade covers it, and a drawing that wants it kept off a cosmetic face has to say so in the gate location, not in the finish note.

Every feature on a cavity has a size in micrometers. The finish grade, the coating, the vent and the texture all live in the same few tens of micrometers, and they interact.

Writing a Finish on the Drawing

A finish note has four parts. The grade, for example SPI B-2, names the method and result class. Next, the face names where it applies, and the texture standard and depth, if a texture is used, set the draft. And the reference, a sample plate or a first article, settles disputes about appearance.

Table 3. Finish notes and the question each one answers
Part of the note Example Question answered
Grade SPI A-2 Which finishing method and result class
Face cosmetic face only Where the grade applies
Texture and depth named texture at 0.002 in (0.05 mm) How much draft the wall carries
Reference approved sample plate What the buyer compares the part against
Maintenance restored at cleaning What happens as the tool wears

A short worked case shows the four parts together. Picture a polycarbonate display cover with one clear window face and four opaque side faces. The note reads: window face SPI A-2, side faces SPI C-1, no texture, reference the approved sample plate, finish inspected at each cleaning. Under that note the window follows the Grade #6 diamond buff row of Table 1, the sides follow the 600 stone row, and the plate decides any argument that the Ra column cannot.

Anyone who writes only “high gloss” has left every part of the note open. A grade, a face and a reference close most of it.

An SPI grade is the shortest word in a drawing, and the one most often left out. For runs of a few to a few thousand parts, low-volume injection molding is the working form of bridge production.

Sources and Further Reading

Request an Injection Molding Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Injection Molding chosen.

Request a Quote