The 20 mm screw on ARBURG’s ALLROUNDER 370 A melts 2.8 kg/h of PA 6.6, and the 40 mm screw on the same 600 kN press melts 12.5 kg/h. A part that needs 30 g every 26 seconds, about 4.2 kg/h, starves the small screw and sits lightly on the large one, and no amount of cooling skill changes that. Cycle time and plasticizing rate have to be read together.
Cycle time turns a quantity into hours on a press, and it is built from a handful of intervals, each with a different owner: the resin, the part’s wall, the tool’s metal, the press. A buyer who understands the intervals can read a supplier’s cycle claim, spot the one that is padded, and see why a part that molds in 30 seconds in steel may or may not mold in 30 seconds in an aluminum bridge tool.
What Sets Cycle Time and Parts per Hour
A molding cycle is a loop of seven moves: the mold closes, the cavity fills, the pack and hold phase runs, the part cools, the mold opens, the part is ejected, and the screw recovers for the next shot. Recovery runs while the part cools, which is why DuPont’s nylon guide asks for screw speeds adjusted so that screw retraction time is shorter than the cooling phase. If recovery is shorter than cooling, it adds nothing to the cycle.
Parts per hour follow from the loop. One hour is 3,600 seconds, so shots per hour at 100 % uptime are 3,600 divided by the cycle time in seconds, and parts per hour are shots multiplied by the cavity count. Real uptime is lower, because the press stops for lot changes, inspections, purges and tool cleaning. A supplier quoting parts per hour should say whether the figure is cycle arithmetic or a measured run.
The intervals belong to different parts of the system.
Fill and pack are set by the resin and gate. Cooling is set by the wall, the resin and the tool metal. Open, eject and close are set by the press and the part’s shape. This division is the basis of the table below.
| Interval | Set mainly by | Evidence in the makers’ documents |
|---|---|---|
| Fill | Resin viscosity, gate size, wall thickness | Nylon fills in 1 to 3 s in thin sections (DuPont); a 1.5 to 2.0 mm wall change gives 50 to 100 % more flow length in Makrolon TC (Covestro) |
| Pack and hold | Part thickness, gate freeze | Hold time found by weighing parts; packing time per mm rises with thickness (DuPont) |
| Cooling | Wall thickness, resin, tool conductivity | Thick parts cool much more slowly (DuPont); aluminum conducts 4 to 5 times as well as P-20 (Arconic) |
| Recovery | Screw speed and back pressure | Retraction time shorter than cooling (DuPont) |
| Open, eject, close | Press, stroke, part shape | Dry cycle time is a published press figure (ARBURG) |
The interval to question is the one that the part does not need. Extra cooling on a crystalline resin or extra hold after the gate has frozen add seconds without adding quality.
Reading the Cycle in a Real Trial
DuPont’s Delrin tips sheet gives one of the few published sets of cycle times next to the dimensions those cycles produced, for a wear-test sample part measured on its outside diameter. Table 2 adds the shots per hour each cycle implies at one cavity and full uptime.
| Trial | Packing, s | Cooling, s | Cycle, s | Shots per hour | Outside diameter, mm |
|---|---|---|---|---|---|
| 1 | 5 | 24 | 39 | 92 | 49.48 ± 0.2 |
| 2 | 10 | 7 | 26 | 138 | 49.48 ± 0.7 |
| 3 | 15 | 2 | 26 | 138 | 49.61 ± 0.02 |
| 4 | 15 | 15 | 41 | 88 | 49.76 ± 0.07 |
Trials 2 and 3 have the same 26 second cycle, and only one of them is good. Trial 2 spent its time on a 7 second cooling with a 10 second pack, which left the part under-packed and its diameter varying by ±0.7 mm. Moving 5 seconds from cooling to packing, trial 3 cut the spread to ±0.02 mm. The cycle did not change and the quality did.
A buyer reading a supplier’s cycle time learns little from the total alone. The same total can come from a tight process or a loose one. Pack time and cooling time behind the total are the part of the number that tells whether the process was optimized or just shortened.
The sheet’s explanation is specific to a crystalline resin. Once packing has been set correctly, DuPont says, acetal is solid and fully crystallized and needs no further cooling, so the part can leave hot and finish cooling in the open. That makes the whole cycle shorter than for amorphous resins, which pack briefly but then wait through a long cooling stage.
Cooling Time, Wall Thickness and Tool Metal
For most parts, cooling is the biggest block of the cycle, and it grows quickly with wall thickness. DuPont observes that thick parts cool far more slowly than thin ones, since thermoplastics conduct heat poorly.
K. A. Stelson’s paper on cooling times for injection molding reviews the published formulae and reports that many contain errors accepted for decades.
It also says that ejection can be based on either mid-plane or average temperature and that thin and thick parts deviate from the theory’s assumptions.
A buyer quoting from a formula should expect the press to differ from it. The trial record, with measured pack and cooling times, is the number to carry into the next order.
The metal in contact with the part changes the rate. Arconic puts the conductivity of aluminum at 4 to 5 times that of P-20 steel, and thyssenkrupp’s table gives QC-10 at 159 W/mK (92 Btu/ft/hr/°F) against 29 W/mK (17) for P-20. For a given wall, an aluminum tool pulls heat out through the cavity faster, and the cooling part of a cycle can be shorter than in a steel tool of the same layout. Shortening is not guaranteed, because the heat still has to cross the plastic wall, which is a poor conductor.
The conductivity advantage can be pushed further with copper alloys. MoldMAX’s brochure credits its alloys, at up to ten times the conductivity of tool steel, with cycles shorter by 15 to 50 %, and prints a case of 10 seconds of mold cooling against 25 seconds for the comparison tool. Those are the maker’s own figures for its alloys, and they describe the direction an insert can move the cooling interval, not the cycle of any given part.
The runner is part of the cooling clock too. In a cold runner tool the runner is molded with the part and has to be solid enough to eject, and DuPont’s rule that the effective runner diameter be larger than the molded part thickness means the runner is often the thickest section in the cavity block. Arconic’s fact sheet describes the alternative, a hot half whose cooled plate shields the aluminum tool from the heat of the hot runner, which removes the runner from the cooling interval and adds the isolation and expansion design its sheet describes.
Resin supplies its own limit. Covestro’s thermally conductive polycarbonate loses heat to the mold quickly, and the company warns that high melt temperatures heat the mold locally, which causes sticking and ejection difficulty. An interval saved at the cooling stage can come back as a longer ejection or a cleaning stop.
Material Throughput and Shot Size Set a Ceiling
A press has to melt as much resin per hour as the cycle consumes. Machine makers publish the limit as material throughput for each screw. Table 3 lists the figures ARBURG gives for its ALLROUNDER 370 A, an electric machine with 370 × 370 mm tie bar spacing and 600 kN (65 US tons) of clamping force, in its three EUROMAP injection units 100, 170 and 290.
| Unit and screw | Maximum shot weight in polystyrene | Throughput, polystyrene | Throughput, PA 6.6 | Maximum injection pressure |
|---|---|---|---|---|
| 100 unit, 20 mm screw | 29 g (1.0 oz) | 5.5 kg/h (12.1 lb/h) | 2.8 kg/h (6.2 lb/h) | 250 MPa (36,250 psi) |
| 100 unit, 30 mm screw | 65 g (2.3 oz) | 9.5 kg/h (20.9 lb/h) | 4.9 kg/h (10.8 lb/h) | 139 MPa (20,155 psi) |
| 170 unit, 25 mm screw | 54 g (1.9 oz) | 10 kg/h (22.0 lb/h) | 5.0 kg/h (11.0 lb/h) | 250 MPa (36,250 psi) |
| 170 unit, 35 mm screw | 105 g (3.7 oz) | 16 kg/h (35.2 lb/h) | 8.0 kg/h (17.6 lb/h) | 147 MPa (21,315 psi) |
| 290 unit, 30 mm screw | 97 g (3.4 oz) | 17 kg/h (37.4 lb/h) | 8.5 kg/h (18.7 lb/h) | 250 MPa (36,250 psi) |
| 290 unit, 40 mm screw | 172 g (6.1 oz) | 24.5 kg/h (53.9 lb/h) | 12.5 kg/h (27.5 lb/h) | 153 MPa (22,185 psi) |
The same screw gives different throughput in different resins, so the nylon column is the one to use when the part is nylon. A worked example makes the limit visible: a shot of 30 g (an assumed value for this arithmetic) at the 26 second cycle of Table 2 is 138 shots an hour, or about 4.2 kg/h (9.1 lb/h) of resin. In PA 6.6 the 20 mm screw tops out at 2.8 kg/h and cannot keep that cycle, while the 30 mm screw of the same unit, at 4.9 kg/h, has only a thin margin.
Shot size also sets the other limit, residence time. DuPont’s nylon guide asks that the machine size or screw diameter be picked so the shot weight does not come out too small, and Covestro sets a shot stroke of 2 to 3 screw diameters for its polycarbonate. A press that is far too large for the part keeps resin in the barrel for many cycles, and a press that is too small cannot melt enough to keep the cycle.
The press fits the part when its throughput covers the cycle and its shot is large enough to turn the barrel over. Both limits are in the maker’s data sheet.
The same data sheet shows a trade between pressure and size. Each unit’s small screw reaches 250 MPa of injection pressure and the large screw only 139 to 153 MPa, so a thin-wall part that needs high pressure to fill sits on the small screw and its lower shot weight, while a thick part that needs volume sits on the large one. Picking the screw is a decision about the part, and it is made before the cycle is quoted.
Clamp Force and How Many Cavities Fit
Clamp force limits how many cavities a tool can have. The press has to hold the mold shut against the pressure of the plastic in the cavities, and the force needed is the projected area of the cavities and runner multiplied by the pressure acting on that area. Resin makers give the pressures: DuPont says hold pressure of about 90 MPa for nylon and 75 to 100 MPa of injection pressure for glass-filled grades.
A rough ceiling for a 600 kN press is the clamp force divided by the pressure. At 90 MPa, 600,000 N divided by 90 N/mm² is about 6,700 mm² (10.3 in²) of projected area, including the runner. That is an upper bound, because pressure in the cavity falls below the pressure at the screw as melt flows through the runner and gate, so real cavity pressures are lower and a larger area is possible. A toolmaker uses flow analysis for the final number.
The ceiling matters in a bridge run for two reasons. A tool with many cavities reaches a quantity in fewer shots, which cuts hours of press time. It also asks for more clamp force and a bigger shot, and the sum of both can move the job to a larger press than the part alone would suggest.
The Sequence Behind Lead Time
The cycle accounts for the hours of molding, and lead time is mostly everything before them. Durations for this sequence are not published in the makers’ documents, and they differ with part, tool and queue, so the order is the useful thing to hold.
- A tool is designed and cut, with gates, vents and cooling placed on the drawing.
- The first shots are taken, and the start-up, the transfer point and the melt temperature are established.
- The pack and hold time is found by a part weight study, and the cooling time by measuring parts.
- Corrections are cut into the tool or made in the settings, and the shots are repeated.
- First articles are measured and sent for approval.
- The approved settings are written down and the lots are molded.
Steps 2 to 4 repeat as often as the part needs, and aluminum or soft steel lets those loops run on the same tool metal. A buyer asking for a date should ask how many correction loops the date assumes, and which step is the one still open. Quoted before step 3, a cycle time is an estimate; quoted after it, the number is a measurement, and it can be checked against the pack and cooling times in the trial record.
Cavities, Hours and the Size of a Run
Hours of molding for a quantity follow from the same arithmetic. Quantity divided by cavities gives shots, shots multiplied by cycle time gives seconds, and uptime scales the result. For the 26 second cycle at one cavity, a quantity of 5,000 parts needs at least about 36 hours of molding time at full uptime, and a four-cavity tool at the same cycle needs about 9 hours.
The lot is the other unit that matters in bridge production. A run is rarely molded in a single stretch. Lots are spaced to deliveries, and each restart spends setup shots, a drying check and a purge, so the effective hours are higher than the cycle arithmetic.
- Ask whether parts per hour are given at full uptime or at measured uptime.
- Ask which cavity count and which press the cycle was run on.
- Ask for the pack and cooling times behind the cycle, so that the total can be checked against a part weight study.
- Ask how the cycle changes at each restart.
The answers also expose a common mismatch. A cycle proven on a four-cavity tool at a steady rate is sometimes quoted for a single-cavity bridge tool, or the reverse, and the hours for the quantity change by the cavity count. Any cycle taken from a different resin, a different wall or a different tool metal belongs to that part, not to yours, because each of those moves the cooling interval that makes up most of the total.
The next tool pays when it changes a variable the cycle arithmetic shows. More cavities cut hours until clamp force or shot size stops them, a faster-cooling alloy cuts the cooling interval. Each is a statement about hours and about tools, and none needs a price. A supplier of low-volume injection molding that quotes a cycle with its pack, cooling and cavity count is giving the buyer the data to plan bridge production in hours, and to see when an extra cavity or a second tool is worth asking for.
Sources and Further Reading
- DuPont, Molding tips to optimize production of components made with Delrin acetal homopolymer, Delrin Technical Guide
- DuPont, Zytel and Minlon nylon resins molding guide (GNE-A11218)
- K. A. Stelson, Calculating cooling times for polymer injection moulding, Proceedings of the Institution of Mechanical Engineers, Part B, 217(5), 709-713, 2003 (abstract page, University of Minnesota)
- ARBURG, ALLROUNDER 370 A technical data, TD 526447 (metric edition)
- voestalpine High Performance Metals, MoldMAX plastic tooling alloys brochure
- thyssenkrupp Materials NA, Aluminum and copper mold materials for the plastics industry, CBS 017-04-18
- Arconic, QC-10 mold material, hot runner integration technical fact sheet
- Covestro, Processing information for Makrolon TC polycarbonate grades, COV-202, August 2022