A molded bar of 30 percent glass-filled nylon 66 measures 10,000 MPa (1.45 million psi) in tensile modulus when it is tested dry as molded. Leave the same bar to condition in room air and the same test reads 6,800 MPa (986,000 psi). BASF prints both numbers side by side on its Ultramid A3WG6 LT BK sheet, and the gap of 32 percent is the first thing a buyer should read before drawing a part in this resin.
Nothing is wrong with the material in that gap. Nylon 66 is hygroscopic, the glass fibers carry the stiffness, and the polymer between them softens as it takes up water. What follows is a reading of this grade family as it behaves in injection molding: what the properties are in both conditions, what the molding window is, what the fibers do to the tool, and what the datasheet leaves unsaid.
Properties of 30 Percent Glass-Filled Nylon 66 Dry and Conditioned
PA66 with 30 percent glass is one of the most common reinforced engineering grades, and BASF’s Ultramid A3WG6 LT BK, a laser-transparent black grade whose sheet is dated 09/2026, is a clear example of how the family reads. The sheet names the polymer PA66-GF30 and gives its typical values for uncolored product at 23 °C.
| Property | Dry | Conditioned | Test |
|---|---|---|---|
| Density | 1.37 g/cm³ (0.049 lb/in³) | not stated | ISO 1183 |
| Tensile modulus | 10,000 MPa (1.45 million psi) | 6,800 MPa (986,000 psi) | ISO 527-1/-2 |
| Stress at break | 190 MPa (27,600 psi) | 127 MPa (18,400 psi) | ISO 527-1/-2 |
| Strain at break | 3.6 % | 6.5 % | ISO 527-1/-2 |
| Flexural modulus | 9,270 MPa (1.34 million psi) | 6,500 MPa (943,000 psi) | ISO 178 |
| Flexural strength | 293 MPa (42,500 psi) | 205 MPa (29,700 psi) | ISO 178 |
| Charpy notched impact at 23 °C | 10 kJ/m² (4.8 ft·lb/in²) | 13 kJ/m² (6.2 ft·lb/in²) | ISO 179/1eA |
| Charpy unnotched impact at 23 °C | 88 kJ/m² (41.9 ft·lb/in²) | 100 kJ/m² (47.6 ft·lb/in²) | ISO 179/1eU |
| Heat deflection at 1.8 MPa | 250 °C (482 °F) | not stated | ISO 75-1/-2, HDT A |
| Heat deflection at 0.45 MPa | 260 °C (500 °F) | not stated | ISO 75-1/-2, HDT B |
| Melting temperature | 260 °C (500 °F) | not stated | ISO 11357-1/-3 |
Read the table in pairs. Every strength and stiffness figure falls once water is in the polymer: stress at break loses 33 percent (190 to 127 MPa), flexural strength loses 30 percent (293 to 205 MPa), and flexural modulus loses 30 percent (9,270 to 6,500 MPa). Strain at break and impact energy move the other way, so the conditioned part is softer and tougher at once.
The dry numbers describe a part on the day it leaves the press. The conditioned numbers describe the same part after weeks in ordinary air. A drawing that quotes only the first column is quoting a part that no longer exists by the time it is assembled.
Heat works the same way as water. The heat deflection figure of 250 °C describes a short test on a loaded bar, not long service, and the stiffness of the polymer between the fibers falls as the part warms. A functional test at 23 °C therefore says little about an enclosure that sits warm beside a motor.
Thermal expansion along and across the fibers
Glass fibers lock down expansion in the flow direction far more than across it, by the same orientation that sets the shrinkage figures below. A flat glass-filled part therefore does not grow as a square when it heats, and a fit that crosses the flow needs its own allowance.
Flammability Named Separately
The sheet prints no flame rating for this grade. Anyone who needs V-0 from a nylon names a flame-retardant grade, because glass does nothing for burning behavior. The Zytel molding guide says as much from the other side: flame retardant grades run about 15 °C (25 °F) lower in melt temperature than the reinforced base grades.
Moisture Uptake and Why Part Dimensions Move After Molding
A part leaves the tool nearly dry and starts absorbing water at once. The DuPont molding guide tabulates equilibrium water absorption for unreinforced nylons at 2.5 percent in air at 23 °C and 50 percent relative humidity for PA66, and 7.5 percent in water. A glass-filled grade takes up less, since glass takes no water and the figure scales with the polymer fraction.
The guide states plainly that water absorption causes expansion, and that final dimensions are the sum of two opposing movements: post-mold crystallization shrinks the part while moisture swells it. In a well-molded part of moderate wall thickness, the guide says the swell dominates. A part molded into a cold tool or with thin sections shows the opposite: the shrinkage from post-crystallization is higher than the swell.
For parts that will live in normal air the guide advises conditioning to roughly 3 percent water by weight for unreinforced PA66 and letting the surface moisture evaporate, which leaves about 2.5 percent. It also notes that the time to equilibrium depends on wall thickness, starting moisture and temperature, and its plot of moisture against time runs to 300 days for walls of 1.5, 3.2 and 6.4 mm. A gauge check on a freshly molded sample and a gauge check on a conditioned sample are two different measurements.
- Before molding, the resin is dried. The guide sets the moisture ceiling at 0.2 percent by weight, dryers at a dew point below -18 °C (0 °F), and fresh bags at 2 to 4 hours at 80 °C (175 °F), with an air flow of about 3.7 m³/h per kg/h of resin.
- After molding, a part ejected dry as molded will take up moisture at a rate set by its thickest wall.
- At inspection, the agreement on the drawing says whether a dimension is read dry as molded or after conditioning at 23 °C and 50 percent relative humidity, which is the condition the guide uses for its own shrinkage figures (kept 24 to 48 hours before measurement).
Melt Temperature, Mold Temperature and Hold Pressure for PA66-GF30
BASF’s processing sheet gives the grade’s window, and DuPont’s nylon molding guide adds the settings a grade sheet leaves out.
| Setting | Range | Optimum | Source |
|---|---|---|---|
| Drying | 4 h at 80 °C (176 °F), recommended moisture 0.03 to 0.06 % | not stated | processing sheet |
| Melt temperature | 280 to 300 °C (536 to 572 °F) | 290 °C (554 °F) | processing sheet |
| Mold temperature | 80 to 90 °C (176 to 194 °F) | 80 °C (176 °F) | processing sheet |
| Maximum residence time | 10 min | not stated | processing sheet |
| Peripheral screw speed | 0.3 m/s (59 ft/min) | not stated | processing sheet |
| Back pressure | about 0.3 MPa (50 psi) or none | not stated | molding guide |
| Fill time | 1 to 3 s, slower for thick sections | not stated | molding guide |
Several of these numbers deserve a sentence each. DuPont’s guide runs hotter than BASF’s 80 °C and ties the heat to results: reinforced resins with mold temperatures near 100 °C improve surface finish, mold filling and surface frosting, and dimensional stability. The same guide says a part molded too cold crystallizes later and keeps shrinking after it is out. A part molded cold and then used in a hot vehicle can therefore change size in service.
Screw speed is a glass issue. The guide warns that high screw speeds with glass-reinforced resins break fibers and lose mechanical properties, which is why the processing sheet gives a modest peripheral screw speed of 0.3 m/s and why back pressure sits low. Fast injection, in contrast, is welcome: the guide calls for fill times of 1 to 3 seconds because a quick fill gives a better surface on nucleated, glass-reinforced nylon.
The hold phase deserves the closest look in a bridge tool. The grade sheet prints no hold pressure, so the setter finds it on the first shots, and whether the aluminum tool in the press is rated for that pressure is a question for the toolmaker. The section on tool wear below returns to it.
Gates, wall thickness and where fibers go
For glass nylon the guide recommends gates about 50 percent larger than for unreinforced nylon, though not thicker. It prefers center gating on round parts and full edge gating on thin rectangles under 1.5 mm. For long flow lengths it recommends placing the gate so the melt impinges on a core or wall, which randomizes fiber orientation. Parts should be designed with uniform wall thickness, and thick sections should be cored out.
Fiber Orientation, Shrinkage and Warpage in Glass-Filled Nylon
Molding shrinkage under ISO 294-4 for this grade is 0.45 percent along the flow and 1.09 percent across it. The ratio of more than two to one is the whole story of why glass nylon warps. Fibers line up with the flow, restrict contraction along it and leave the transverse direction to shrink like unreinforced nylon.
The DuPont guide names the causes of warpage: fiber orientation, non-uniform wall thickness, and non-uniform mold temperature, including local overheating of cores and a missing water channel in one area of the cavity. Its remedies are the ones already listed: random fiber distribution through abrupt flow changes, cores that split the melt, multiple gates, and blending to a lower glass content where the end use allows it.
For a 100 mm dimension, the datasheet values predict 0.45 mm of shrinkage along the flow and 1.09 mm across it, a difference of 0.64 mm on a single edge of a flat part before any wall variation is added. Any tolerance written without the flow direction in mind is a tolerance written about the part’s average, which does not exist.
Orientation sets shrinkage. A glass nylon part with one gate and a long flat face shrinks at two different rates in two directions, and the drawing, the tool and the inspection plan should all know which direction is which.
What Glass Does to an Aluminum Injection Tool
Aluminum tooling and glass-filled nylon are used together, and the combination is sensitive in specific places. The maker’s guidance and the tooling trade literature point to the same places.
A trade article from Plastics Technology, written by the vice president of tooling at an aluminum tool shop, describes the pattern. Filled resins wear out the shutoffs and the gate area first. Its recommended remedies are a nickel-boron surface coating of about 0.0002 to 0.0003 in. (5 to 8 µm) that raises surface hardness to 50 to 56 HRC, which takes about three days to apply and can be stripped and recoated when it wears, and steel or other inserts in high-wear areas such as slide-by shutoffs with minimal draft or the gate region when an abrasive resin runs. Inserting an aluminum mold is preferred to welding, because the weld can leave pitting and is softer than the surrounding aluminum.
The same article describes the care that keeps a tool alive: the tool is taken apart and cleaned thoroughly after every run, often every five to seven days of running and sometimes every two to three, and it is cleaned before storage even when the run was short. It cites a multiyear study by a large automaker and other cases in which aluminum tools reached the million-shot mark with proper care, and a four-cavity ABS tool near 200,000 shots. Those cases involved unfilled resin. The article does not give a shot count for glass nylon, and the sources opened for this piece contain none, so no life number is given here for this resin on any alloy.
- Gate area. Fibers carried in a melt at 280 to 300 °C scour the land where the melt speeds up. A worn gate grows, packs differently and moves the shrinkage, so gate dimensions are part of the check at each tool removal.
- Shutoffs and slides. Glass-filled flash is abrasive. Minimal-draft shutoffs are the first places to show wear.
- Cores and ejection faces. Glass-filled resin also rubs the cores and pins it is stripped from, and the tool’s record of those faces belongs in the same wear check as the gate.
- Heat and pressure. The Plastics Technology article warns that excessive temperatures and injection pressures damage aluminum tools quickly through detail shifting and galling, while noting that aluminum’s thermal advantages usually give a wider process window than steel.
A buyer asking for glass nylon in a bridge tool should therefore ask three questions of the toolmaker. The first is whether the gate and shutoff areas are inserted or coated. Next comes the hold pressure the tool is rated for, set against what the first shots need. Last is how gate and shutoff dimensions are checked at each cleaning.
What the Datasheet Leaves Out for This Grade
A datasheet reports molded test bars, and a part is not a bar. Several things stay outside the sheet and need a decision before a purchase order.
| Open item | Why it matters | What closes it |
|---|---|---|
| Part-specific shrinkage | The 0.45 and 1.09 percent figures come from an ISO 294-4 test plaque | T1 sample measured on the actual part |
| Conditioned dimensions | Moisture swells the part after molding | A stated measurement condition on the drawing |
| Fiber orientation in the real part | Sets warpage and direction-dependent strength | Gate location agreed before tool steel is cut |
| Flame rating | The sheet prints none for this grade | A flame-retardant grade named in the order |
| Tool wear by shot count | No shot number is printed for this resin on aluminum | Inspection of gate and shutoffs at each run |
Another gap is color. The sheet’s typical values are for uncolored product while the grade itself is black, and the guide notes that pigments influence shrinkage in semi-crystalline nylons. A black or colored part may not shrink as the natural bar did, and the guide lists pigments among the resin-side causes of shrinkage change.
The molding guide also covers regrind. It advises using rework only as it is generated and limiting it to 50 percent or preferably 25 percent blended with virgin resin, because mechanical properties of reinforced nylon fall with the number of passes. For a bridge run in which the first parts may go to qualification, a clear statement of regrind content in the order protects the property data in Table 1.
- A grade is named by its full designation, here Ultramid A3WG6 LT BK, because a suffix names a different version with its own sheet.
- A condition is named for every dimension and property: dry as molded, or conditioned at 23 °C and 50 percent relative humidity.
- A flow direction is named for every critical dimension.
Glass-filled nylon 66 gives a stiff, heat-resistant part from a tool made of aluminum, provided that the drawing carries the moisture condition and the flow direction and that the gate is treated as a wear item. For parts in the range of a few to a few thousand pieces, low-volume injection molding is the usual form of bridge production.
Sources and Further Reading
- BASF, Ultramid A3WG6 LT BK Product Information, 09/2026
- BASF, Ultramid A3WG6 LT BK Processing Data Sheet, 09/2026
- DuPont, Zytel and Minlon Nylon Resins Molding Guide, processing summary, drying, shrinkage, post-mold shrinkage, warpage, water absorption, regrind
- Scott Lammon, Phoenix Proto Technologies, Aluminum Injection Tooling: How to Use and Maintain It, Plastics Technology
- ISO, ISO 294-4:2018 Plastics, Injection moulding of test specimens of thermoplastic materials, Part 4, Determination of moulding shrinkage, abstract and status