GateCavityAcetal

Injection Molding Shrinkage Along and Across the Flow by Material

Molding shrinkage read by direction and condition for three resins, with the process settings that move it and the way a first sample turns it into a cavity allowance.

An injection molded flat plastic plate beside the polished mold insert it was shot from, the plate slightly smaller.

A 60 by 60 mm plate, 2 mm thick, gated along one edge, is the part that most of the plastics industry measures shrinkage on. DuPont’s nylon guide describes it as a fan-gated rectangular plate of 60 by 60 by 2.0 mm, measured at 23 °C in the dry-as-molded state after 24 to 48 hours at 23 °C and 50 percent relative humidity. Every shrinkage figure printed on a datasheet for the resins in this piece comes from a plaque of that kind, and no real part looks like it.

The figure on the sheet is therefore a start, not a tolerance. Below, the values for three resins are read, the ISO test is defined, what the ISO test measures, show process settings that move the number are shown with their size, and the result becomes a cavity allowance for an aluminum tool, with the conditions that belong to each value.

Shrinkage of Polycarbonate, Glass-Filled Nylon 66 and Acetal Along and Across the Flow

ISO 294-4:2018 sets out the method for measuring mold shrinkage and post-mold shrinkage of injection molded thermoplastic test specimens, parallel and normal to the direction of melt flow. Resin makers print the result in two lines, one per direction.

Table 1. Molding shrinkage printed on three maker datasheets, with the same value converted to a 250 mm (10 in) length
Resin and sheet Along the flow Across the flow Along, on 250 mm Across, on 250 mm Test conditions on the sheet
Polycarbonate, Makrolon 2407 0.65 % 0.70 % 1.63 mm (0.064 in) 1.75 mm (0.069 in) ISO 294-4, 60 by 60 by 2 mm, hold at 500 bar (50 MPa)
Nylon 66 with 30 % glass, Ultramid A3WG6 LT BK 0.45 % 1.09 % 1.13 mm (0.044 in) 2.73 mm (0.107 in) ISO 294-4
Acetal homopolymer, Delrin 500P 2.0 % 1.9 % 5.0 mm (0.197 in) 4.75 mm (0.187 in) ISO 294-4

Covestro adds a second line for polycarbonate: a practical range of 0.5 to 0.7 percent for parts, under ISO 2577, based on general practical experience, with a note that production values vary with part and mold design and with molding conditions. On a 250 mm length that range is 1.25 to 1.75 mm, a spread of 0.5 mm that no datasheet value removes.

Three patterns are visible in Table 1. Acetal shrinks most, because it crystallizes by almost 60 percent and loses volume as it does, a mechanism DuPont’s tips describe with 11 percent of volume lost to crystallization and a further 7 percent to cooling. Glass-filled nylon shrinks least along the flow and most across it, because the fibers lie along the flow and hold the polymer there. And polycarbonate, an amorphous resin, shrinks little and almost equally in the two directions.

Read the two columns together. A material with a small gap between along and across keeps its shape when it shrinks, and a material with a large gap changes shape.

Because the shrinkage numbers describe a plaque, a part’s own value is found by measurement, and the printed pair is the first estimate on which a toolmaker starts. The estimate is better for a flat, evenly walled part gated at one edge, which resembles the plaque, and worse for a part with deep ribs, thick bosses or several gates.

What the test conditions bring with the number

A shrinkage value belongs to the conditions that produced it. Makrolon’s test specimens are molded at a melt temperature of 280 °C, a mold temperature of 80 °C and an injection velocity of 200 mm/s, while the sheet’s processing recommendation for production is a standard melt of 300 °C and a mold of 80 to 120 °C. BASF’s processing sheet for its glass nylon gives a melt of 290 °C and a mold of 80 °C as optimal. A production part molded at its own best conditions is not molded at the conditions behind the printed shrinkage.

What ISO 294-4 Measures and What It Excludes

The abstract of ISO 294-4 states that the standard specifies a method for determining mold shrinkage and post-mold shrinkage of injection-molded test specimens of thermoplastic materials, and that mold shrinkage as defined excludes the effects of humidity, which belong to post-mold shrinkage and total shrinkage. It adds that the value is free shrinkage, the maximum value of any restricted shrinkage. The standard is edition 3, published in December 2018 by the technical committee for thermoplastic materials, ISO/TC 61/SC 9, and its status was confirmed in 2024.

Two consequences follow for a buyer. The printed value is the upper limit for a part that shrinks freely, and a real part has ribs, bosses and walls that restrain it. A restrained feature shrinks less than the printed value, which the DuPont guide shows in its figure comparing free and restrained shrinkage. And the printed value says nothing about water, so for nylon it describes the dry state only.

  • Free shrinkage is a ceiling. A long clear span shrinks close to it, and a feature held between walls shrinks less.
  • Humidity is outside the number. A nylon part takes up water after molding, 2.5 percent at equilibrium in 23 °C and 50 percent relative humidity for unreinforced PA66 in DuPont’s guide, and swells after the shrinkage was measured.
  • Direction is inside the number. The two lines on the sheet are the along and across values, and a feature at an angle sits between them.

Mold Temperature, Wall Thickness and Hold Pressure and What They Do to Shrinkage

DuPont’s nylon guide gives the clearest published account of what moves the number in a semi-crystalline resin. The central statement is that crystallization of the polymer and thermal contraction both happen as the part cools, and that process settings change how much of each occurs.

  • Mold temperature. Shrinkage increases with mold temperature, because a hot mold lets the polymer crystallize more fully, and the guide gives the same effect in reverse for post-mold shrinkage, which is high for a part molded cold and low for a part molded hot.
  • Wall thickness. Shrinkage increases with thickness, because a thick section cools slowly, with a low thermal conductivity of plastics in the guide’s words.
  • Hold pressure. The highest possible holding pressure is applied to diminish shrinkage, usually around 90 MPa, and a variation of 10 MPa gives about 0.1 percent variation in shrinkage.
  • Hold pressure time. Shrinkage reaches a minimum at the correct hold pressure time, which is also where part weight reaches its maximum, so weighing parts at stepped hold times finds the right setting.
  • Gate. Hold time is effective only when the gate dimensions are adequate and the gate freezes at the time the part has crystallized, not before.
Table 2. Size of the shrinkage effect of process settings, using the DuPont guide’s 0.1 percent per 10 MPa figure and the polycarbonate range from Covestro
Setting or condition Change in shrinkage Length change on 100 mm Length change on 4 in
Hold pressure varies by 10 MPa (nylon) about 0.1 % about 0.10 mm about 0.004 in
Hold pressure varies by 20 MPa (nylon) about 0.2 % about 0.20 mm about 0.008 in
Practical range for polycarbonate parts 0.5 to 0.7 % 0.50 to 0.70 mm 0.020 to 0.028 in
Along and across gap, glass nylon 0.64 points 0.64 mm 0.025 in
Along and across gap, polycarbonate 0.05 points 0.05 mm 0.002 in

Table 2 is arithmetic on the printed figures. The pressure rows scale the guide’s rule linearly, which the guide gives for a 10 MPa step and which is an extrapolation at 20 MPa. Rows for the direction gap are differences of the sheet’s own lines.

Packing time and part weight as a shrinkage meter

The method in the DuPont guide for finding the hold time is a bench method. Several hold times are set 0.5 to 1.0 second apart, the parts are weighed after removing runner and sprue, and the correct time sits where weight stops rising. Total cycle time, the guide adds, is kept constant during the trial so that melt temperature stays constant. The same idea works for acetal, where DuPont’s tips show that part weight rises with packing time until it levels off and that the packing time per millimeter grows with thickness.

For a buyer, this means that a shrinkage figure on a first sample is only meaningful if the hold time is on the weight plateau. A part from a short hold shrinks more, and its dimensions will not match the later production parts.

Post-Mold Shrinkage and Moisture Change in Nylon

A nylon part continues to change after it leaves the press. The DuPont guide defines post-mold shrinkage as the dimensional change of a molded part measured at 23 ± 2 °C after annealing for a stated time at a stated temperature, and it finds that annealing shrinkage decreases with mold temperature and is larger for thin walls. Parallel to this, water absorption causes expansion. In a well-molded part of moderate wall thickness the swell outweighs the post-crystallization shrinkage, and in a part molded cold or thin the shrinkage wins.

For glass-filled nylon 66 the guide frames the swell: unreinforced PA66 reaches 2.5 percent water at equilibrium in 23 °C and 50 percent relative humidity, and a glass grade takes up less, in proportion to its polymer. The grade sheet gives no dimensional change for this water uptake, and the guide’s curve of dimensional change against moisture is for unreinforced nylon 66, so the figure for the glass grade is left unstated here.

  • Dry as molded. A part measured soon after molding sits at the shrunken, dry dimension.
  • Conditioned. A part conditioned to equilibrium sits larger by the swell, in a direction-dependent amount for glass-filled nylon.
  • Annealed. A part annealed after molding sits smaller by the post-mold shrinkage, less for hot-molded and thick-walled parts.

Acetal and polycarbonate carry far less of this effect. Delrin 500P absorbs 0.2 percent water at 23 °C and 50 percent relative humidity in Delrin’s Module III, and Makrolon 2407 absorbs 0.12 percent, both under ISO 62, against several percent for nylon. For those resins the shrinkage and the thermal expansion carry most of the dimensional story.

Turning a Shrinkage Range Into a Cavity Allowance

A toolmaker cuts the cavity larger than the part, and the arithmetic is cavity equals part divided by one minus the shrinkage fraction. For polycarbonate on a 100 mm dimension, 0.6 percent gives a cavity of 100.60 mm. If the part then shrinks 0.5 percent it measures 100.10 mm, and if it shrinks 0.7 percent it measures 99.90 mm, a band of 0.2 mm that comes only from the range on the sheet.

For glass-filled nylon the allowance is set in each direction, and the arithmetic gives a cavity of 100.45 mm along the flow and 101.10 mm across it on a 100 mm part. If hold pressure then drifts by 10 MPa, each figure shifts by about 0.1 mm, and the part that drifted measures 0.1 mm off in both directions.

For acetal the allowance is large, 102.04 mm for 100 mm along the flow, and the hold time has to be on the plateau so that the 2 percent is the shrinkage that actually occurs.

A shrinkage figure on a datasheet gives the starting point of the allowance. The first samples give the number the cavity is corrected to.

A Worked Case on a Flat Glass-Filled Nylon Cover

Take a cover 120 mm long and 80 mm wide, gated at one short end so that the flow runs along the 120 mm length, molded in the 30 percent glass nylon of Table 1. The sheet gives 0.45 percent along the flow and 1.09 percent across it.

With an allowance cut for each direction, the cavity is 120.54 mm by 80.88 mm, and the part comes out at 120 by 80 mm. If a single allowance of 0.7 percent is used for both directions, a plausible figure for an unreinforced resin, the cavity is 120.85 mm by 80.56 mm. The part then comes out at 120.30 mm along the flow, 0.30 mm too long, and 79.69 mm across it, 0.31 mm too short. This error belongs to the allowance, and no process drift is involved in it.

On top of that comes the process. A 10 MPa change in hold pressure moves each dimension by about 0.1 percent, which is 0.12 mm on the 120 mm length and 0.08 mm on the 80 mm width. Those two movements are smaller than the single-allowance error and larger than the tolerance a close-fitting lid would carry.

  • A wrong allowance is a systematic error, found on the first sample and corrected in the cavity.
  • A process drift is a random error, controlled on the press by a fixed hold pressure, a fixed hold time and a fixed mold temperature.
  • An orientation effect is a shape error, controlled by gate position and a lower glass content where the end use allows.

The three kinds of error are corrected in different places, and a buyer who sees all three in one first-sample report knows which one the toolmaker, the molder and the designer each owns.

Setting Shrinkage Expectations on an Aluminum Bridge Tool

DuPont’s guide recommends prototype molds for complicated precision parts. It says shrinkage values are intended as approximate guides because of the influence of the factors above, and that prototype molds give more accurate dimensional data. An aluminum bridge tool is that prototype mold in the guide’s sense, and the first samples from it are the shrinkage data for the part.

A short sequence turns this into practice.

  1. The toolmaker states the allowance in each direction and the datasheet figure behind it.
  2. The first samples are molded with the hold time on the weight plateau and the mold temperature set to the production value.
  3. The samples are measured at 23 °C after a stated time, and nylon samples are measured in the stated moisture state.
  4. The cavity is corrected where the allowance missed, and the correction is recorded with the process conditions.
  5. The corrected conditions go on the setup sheet, so the production run repeats them.

Aluminum’s thermal conductivity gives a faster cooling path, and the trade literature on aluminum tools notes that the process window is typically larger than steel’s, with a warning against excessive temperature and pressure that damage the tool. Since the sources opened for this piece contain no shrinkage comparison between aluminum and steel tools for the same part, none is claimed.

The same cover in polycarbonate would show almost no direction effect, so its first sample reads mostly as one number, and the same cover in acetal would show a large single allowance of about 2 percent. Each resin asks for its own first-sample reading. A shrinkage figure read with its direction, conditions and moisture state is a usable number. For parts in the range of a few to a few thousand pieces, low-volume injection molding is the working form of bridge production.

Sources and Further Reading

Request an Injection Molding Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Injection Molding chosen.

Request a Quote