MoistureBarrelHot Runner

Acetal Homopolymer Injection Molding Properties and Gate Rules

Delrin 500P read from the maker's sheet and molding tips: why acetal shrinks and needs a packed gate, how hot the melt may run, and what to check on an aluminum tool.

Injection molded acetal parts in white and black, a cam, a clip and a small gear, a tiny gate mark on each.

DuPont puts the difference between the density of acetal homopolymer melt and the density of the solid at 18 percent. Its Delrin molding tips print both numbers, 1.17 g/cm³ for the melt and 1.42 g/cm³ for the solid, and that gap is the reason a molded acetal part either carries the right gate or carries a void in its thickest section.

Acetal, written POM in the ISO system, is chosen for gears, clips, sliding guides and housings that need to hold shape under load. The sections below read Delrin’s published data for Delrin 500P NC010, a medium-viscosity homopolymer, with its molding guide and molding tips, then show what that means for a bridge tool in aluminum.

Delrin 500P Properties in Metric and Inch Units

Delrin 500P NC010 is a medium-viscosity acetal homopolymer, and Delrin prints its ISO values as the reference beside 500CPE on its own product data sheet. The grade has a melt mass-flow rate of 15 g/10 min at 190 °C and 2.16 kg under ISO 1133. Delrin’s Design Guide Module III adds a longer ISO table for the same grade, and Table 1 takes each row from one of the two.

Table 1. Delrin 500P NC010 typical ISO values, from Delrin’s product data sheet and Design Guide Module III
Property SI value Inch or US value Test
Density 1.42 g/cm³ 0.0513 lb/in³ ISO 1183, data sheet
Tensile modulus 3,100 MPa 450,000 psi ISO 527, data sheet
Yield stress 71 MPa 10,300 psi ISO 527, data sheet
Yield strain 17 % 17 % ISO 527, data sheet
Nominal strain at break 30 % 30 % ISO 527, data sheet
Flexural modulus 2,870 MPa 416,000 psi ISO 178, Module III
Charpy notched impact, 23 °C 9 kJ/m² 4.3 ft·lb/in² ISO 179/1eA, data sheet
Charpy notched impact, -30 °C 8 kJ/m² 3.8 ft·lb/in² ISO 179/1eA, data sheet
Charpy unnotched impact, 23 °C 310 kJ/m² 148 ft·lb/in² ISO 179, Module III
Heat deflection at 1.8 MPa 93 °C 199 °F ISO 75, Module III
Heat deflection at 0.45 MPa 162 °C 324 °F ISO 75, Module III
Melting temperature 178 °C 352 °F ISO 11357, data sheet
Water absorption at 23 °C and 50 % RH 0.2 % 0.2 % ISO 62, Module III
Water absorption, saturation at 23 °C 1.4 % 1.4 % ISO 62, Module III

Three rows deserve a closer look. Notched Charpy at 9 kJ/m² is low next to the unnotched 310 kJ/m², which says the polymer is tough when smooth and sensitive to a sharp corner. The water absorption of 0.2 percent at 23 °C and 50 percent relative humidity is a fraction of what nylons take up, which is the main reason acetal parts hold dimension in damp air. And the table has no long-term stiffness at all: Delrin’s design guide plots creep as curves, from which the tensile creep modulus for a given stress and time is read, and a part under constant load is designed on that long-term value.

Acetal is stiff, slippery and nearly insensitive to humidity. It is also notch-sensitive and creeps under steady load, so the fillet radius and the load duration belong in the design before the grade is chosen.

Module III gives the linear thermal expansion as 0.91E-4 per K in the flow direction and 0.93E-4 per K across it between 23 and 55 °C. A 100 mm length grows about 0.09 mm for every 10 °C, which is large for a part held to hundredths, and it means a gauge at a different temperature gives a different reading.

Why Acetal Shrinks Two Percent and Needs a Packed Gate

Molding shrinkage for 500P is 2.0 percent in the flow direction and 1.9 percent across it under ISO 294-4. That is more than three times the shrinkage of polycarbonate and, unlike glass-filled nylon, nearly the same in both directions. The cause is crystallinity. DuPont describes acetal homopolymer as one of the most crystalline of the semi-crystalline thermoplastics, at almost 60 percent crystalline, with a solid density of 1.42 g/cm³ against 1.17 g/cm³ for the melt in the molding tips.

A pressure-volume diagram in DuPont’s tips shows two stages. Crystallization takes about 11 percent of the volume, and cooling the solid takes a further 7 percent, which DuPont puts at about 2 percent in linear dimensions. The first stage can be fed with more melt through the gate while the gate is open, and the second cannot. A gate that freezes before the part has crystallized leaves the part to pull its own volume inward as voids and uncontrolled shrinkage.

Another piece of data from the same document: DuPont states that when the part thickness changes, the optimum packing time changes with it, but not in proportion. Its plot shows packing time per millimeter rising as thickness rises. The molding guide’s rule of 8 s per mm, based on a 3 mm wall, is therefore an average, and DuPont’s plot puts thicker walls above it per millimeter.

Melt Window, Hot Runner Temperature and the Foaming Test

Acetal punishes heat in a way that nylon and polycarbonate do not, and DuPont gives the numbers that matter.

Table 2. Processing window for Delrin standard grades from Delrin’s molding guide
Setting Range Optimum US units
Drying As a rule none; 2 to 4 h at 80 °C where moisture is above 0.2 % not stated 176 °F
Melt temperature 210 to 220 °C 215 °C 410 to 428 °F, optimum 419 °F
Hot runner 190 °C at most 190 °C 374 °F
Mold temperature 80 to 100 °C, up to 120 °C for high precision not stated 176 to 212 °F
Hold pressure 60 to 110 MPa, depending on the grade not stated 8,700 to 16,000 psi
Hold pressure time 8 s per mm of wall, based on a 3 mm wall not stated 8 s per 0.04 in

The tips quote a recommended melt temperature of 215 °C with a tolerance of 5 °C, at which standard grades stay stable for more than 30 minutes. A plot of melt temperature against maximum residence time in the barrel ties the two: the higher the melt, the shorter the time the resin can sit. Nozzle and hot runner temperatures are set to 190 °C because the outer skin of molten polymer stays still against the metal wall, and higher settings degrade after a few hours of running and call for more frequent cleaning.

The foaming test on a purge

DuPont describes a qualitative check that a floor can make in a minute. A molten purge is dropped into water. Sound melt carries no gas bubbles, is denser and sinks, and its section shows only the matte voids of crystallization. Degraded melt carries bubbles and floats, and its section shows large shiny voids from degradation gas. The test is particularly useful with colorants, because some masterbatch pigments and additives are known to degrade acetal and should be avoided. A resin that foams when molten deposits on the mold quickly and speeds deposits on the screw, which can lead to black specks.

  • Pigment. The color grade and its masterbatch are agreed with the resin maker before the order, not on the day of the first shot.
  • Purge. The foaming test is run on the purge before the first part is kept.
  • Residence time. The melt temperature and the time in the barrel are read together against the DuPont plot, because the allowed time shrinks as the melt gets hotter.

DuPont also gives a firm warning that acetal is never mixed or processed with halogenated polymers or chemicals such as PVC, nor with flame retardant resins. The HCl or HBr they give off causes fast degradation of the acetal. A tool, barrel or hot runner that last ran a flame-retardant or PVC grade has to be cleaned before acetal runs in it.

Tunnel Gates and Packing Rules for a Semi-Crystalline Resin

The most useful page in DuPont’s tips is the comparison of a tunnel gate and a conical gate. Amorphous resins fail by over-packing, and a conical gate suits them. Acetal fails by under-packing, because it crystallizes in a narrow gate tip before packing is complete, and the document states that poor packing cuts mechanical performance by up to 30 percent and causes warpage and uncontrolled shrinkage.

For the tunnel gate DuPont gives these criteria:

  • The gate sits in the thickest area of the part.
  • The gate diameter d is at least half the part thickness T.
  • The gate length is under 0.8 mm (0.03 in), so the gate does not freeze early during packing.
  • The tunnel diameter D next to the gate is at least T plus 1 mm.

For a 3 mm wall these rules give a gate of at least 1.5 mm diameter, a land under 0.8 mm long and a 4 mm tunnel behind it. A designer who draws a 0.8 mm pin gate on that wall has drawn a gate that freezes first.

DuPont also gives a rule for ejection that surprises people used to amorphous resins. Eject the part hot and let it cool outside the mold, on a conveyor, because once packing is finished the whole part is crystallized and solid, and a hot part constrained in a cooling mold shrinks unevenly. Ejecting into a box or bag causes a temperature gradient through the container and may cause dimensional differences. The data behind this advice is read in the companion piece on acetal dimensional precision.

Reading the Creep and Hardness Data for a Sliding or Snap-Fit Part

A buyer who orders acetal for a gear, a guide or a snap-fit clip is buying a short list of numbers from Table 1, and each of them carries a condition that changes how it is used.

The tensile modulus of 3,100 MPa is a short-term value at 23 °C, and the stress-strain behavior that gives it is the one from the ISO 527 bar. A clip that stays deflected for months loads the material in relaxation, and Delrin’s guide reads the relaxation modulus for that case from its own curves, a lower value than the short-term figure, so a clip designed on the short-term number relaxes in service. The yield strain of 17 percent sets the upper limit of what a snap fit may take in a single assembly, and a repeated assembly is judged on a lower strain that the sheet does not state.

The unnotched Charpy result of 310 kJ/m² and the notched 9 kJ/m² show the scale of notch sensitivity, a factor of more than 30. A sharp internal corner at the root of a snap hook or a gear tooth acts as a notch, and the radius on the drawing is worth more than a grade change. The hardness entry, Rockwell R 120, describes a surface that resists indentation under a gear mesh. It does not describe wear, which the friction figure only begins to cover. The first lot of an acetal gear or slide is often cut as machined plastic from POM rod, and those parts test the fit well while their creep and wear come from extruded stock rather than from a molded part with its own orientation.

  • Gear and guide. Dimensional stability in damp air from the 0.2 percent absorption, creep from the long-term curves, and the tooth root radius.
  • Snap fit. Strain kept well inside the 17 percent yield strain, with the assembly count agreed.
  • Housing with a screw boss. The long-term modulus again, plus an expansion near 0.9E-4 per K against the screw’s own expansion.

Acetal numbers come with a time and a notch attached. The same bar reads 310 kJ/m² smooth and 9 kJ/m² notched, and its stiffness under a steady load is read from creep curves, not from the table.

Heat, Flame and Fit Notes From the Maker’s Data

The heat deflection temperature under 1.8 MPa is 93 °C by the ISO method and 124 °C by ASTM D648 on annealed specimens, both in Module III. The molding guide treats annealing as occasional, at 160 °C for 30 minutes plus 5 minutes per millimeter of wall, so a 4 mm wall takes 50 minutes. It warns that annealing a part molded in a cold mold, below 80 °C, leads to high post-molding shrinkage and uncontrolled deformation, and it can warp a complex part that sits unsupported at 160 °C, so trials come first.

The flame rating is UL 94 HB at 0.75 mm and at 1.5 mm, with a limiting oxygen index of 21.2 percent and a comparative tracking index of 600, all in Module III for 500P NC010. Acetal is therefore a good electrical insulator that burns, and a part that needs a flame class above HB needs another resin.

Module III also lists a Rockwell hardness of R 120 and a dynamic coefficient of friction of 0.30 without lubricant for the P grades. These support the choice for sliding parts, and the guide’s curves for modulus against temperature and for creep are what a designer asks for by name.

Acetal in an Aluminum Injection Tool

The mold temperature of 80 to 100 °C and the hold pressure of up to 110 MPa suit a steel tool, and an aluminum tool is not an exception, but it is not a free choice either. A trade article on aluminum tools states that excessive temperature and injection pressure damage the tool through detail shifting and galling, and that aluminum’s thermal conductivity usually widens the process window against steel. Because the resin carries no glass, the abrasive wear on gates and shutoffs that glass nylon causes is not part of the picture, and the same article reports aluminum tools above 200,000 shots on unfilled ABS and cases above a million shots with strong maintenance procedures.

Two practical points follow for an acetal tool. First, a gate cut to the tunnel rules above is a precise feature, 0.8 mm long at most, and its wear is the first thing that changes the packing, so the gate land is checked at each cleaning. Second, the tool runs at 80 to 100 °C and DuPont asks for the part to be ejected hot, so the ejection system and the receiving conveyor are part of the dimensional plan.

Table 3. Items the acetal datasheet leaves open for a buyer
Open item Why it matters What closes it
Homopolymer or copolymer The sheet covers a homopolymer, and copolymer grades have separate sheets The grade named in full on the order
Color and masterbatch Some pigments degrade the melt The color and its masterbatch cleared with the resin maker
Wall thickness above the thin range Hold time per millimeter rises with thickness The packing time found on the first shots
Annealing Occasional, at 160 °C for 30 min plus 5 min per mm A decision on the drawing, with the dimension read after it
Tool wear at the gate Hold pressure up to 110 MPa on aluminum An agreed pressure limit and a gate check

Acetal gives a stiff, low-friction part with little moisture growth, from a tool of aluminum, on the condition that the gate packs the part and the melt never gets hotter or longer in the barrel than the DuPont plot allows. For runs of a few to a few thousand parts, low-volume injection molding is the working form of bridge production.

Sources and Further Reading

Request an Injection Molding Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Injection Molding chosen.

Request a Quote